{"id":794793,"date":"2026-11-23T13:06:15","date_gmt":"2026-11-23T13:06:15","guid":{"rendered":"https:\/\/www.europesays.com\/ie\/794793\/"},"modified":"2026-11-23T13:06:15","modified_gmt":"2026-11-23T13:06:15","slug":"mapping-safety-zones-as-lithium-ion-batteries-degrade-to-improve-safety","status":"publish","type":"post","link":"https:\/\/www.europesays.com\/ie\/794793\/","title":{"rendered":"Mapping safety zones as lithium-ion batteries degrade to improve safety"},"content":{"rendered":"<p>Degradation measurements<\/p>\n<p>To prepare degraded cells for thermal abuse failure experiments and validate our degradation submodel, degradation measurements were conducted on LG M50T cells at different degradation temperatures, covering a full SoC window from 0% to 100%. Eight fresh cells were tested, with three cycled at 10\u2009\u00b0C, three at 40\u2009\u00b0C and two at 25\u2009\u00b0C. At the outset, the cells were subjected to an initial break-in procedure of five charge\u2013discharge cycles at 25\u2009\u00b0C. Each cycle involved charging at 0.2\u2009C to 4.2\u2009V, followed by a constant voltage phase until the current dropped to C\/100, succeeded by discharging at 0.2\u2009C to 2.5\u2009V. After each cycle, the cells were allowed to rest for 2\u2009h and 4\u2009h. The cells were characterized both at their BoL and after each degradation set through an RPT at 25\u2009\u00b0C. The RPT followed two different procedures: a comprehensive procedure conducted after every even-numbered degradation set, and a concise procedure performed after each odd-numbered degradation set<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 69\" title=\"Kirkaldy, N., Samieian, M. A., Offer, G. J., Marinescu, M. &amp; Patel, Y. Lithium-ion battery degradation: measuring rapid loss of active silicon in silicon&#x2013;graphite composite electrodes. ACS Appl. Energy Mater. 5, 13367&#x2013;13376 (2022).\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#ref-CR69\" id=\"ref-link-section-d420863986e1284\" rel=\"nofollow noopener\" target=\"_blank\">69<\/a>,<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 70\" title=\"Kirkaldy, N., Samieian, M. A., Offer, G. J., Marinescu, M. &amp; Patel, Y. Lithium-ion battery degradation: comprehensive cycle ageing data and analysis for commercial 21700 cells. J. Power Sources 603, 234185 (2024).\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#ref-CR70\" id=\"ref-link-section-d420863986e1287\" rel=\"nofollow noopener\" target=\"_blank\">70<\/a>. Between each step of these procedures, the cells underwent a constant current\u2013constant voltage charging process at 0.3\u2009C up to 4.2\u2009V, maintaining at 4.2\u2009V until the current dropped to C\/100, followed by a 1-h rest period. The cells after having reached their EoL were stored at 10\u2009\u00b0C with 30% SoC before thermal abuse failure measurements. Seven additional cells were degraded for measuring the safety zones and their boundaries under three selected conditions: 0.3\u2009C\/1\u2009C at 25\u2009\u00b0C (base case), 0.7\u2009C\/1\u2009C at 10\u2009\u00b0C (case 1) and 0.3\u2009C\/1\u2009C at 40\u2009\u00b0C (case 3). For each condition, we measured the states on the safety zone boundaries at the BoL and the 3rd RPT after 156 cycles (after the predicted turning point on the safety boundaries), using two cells per point to balance statistical reliability and experimental time constraints. The state on the safety zone boundaries at the EoL was measured for the base case conditions after 1,170 cycles.<\/p>\n<p>DM analysis<\/p>\n<p>The contributions of different DMs including LLI, loss of active material at the negative electrode (LAMNE) and loss of active material at the positive electrode (LAMPE) were identified for model validation. We used an established diagnostic method based on open-circuit voltage (OCV) fitting to quantify these DMs, which is a nondestructive method detailed in our previous work<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 69\" title=\"Kirkaldy, N., Samieian, M. A., Offer, G. J., Marinescu, M. &amp; Patel, Y. Lithium-ion battery degradation: measuring rapid loss of active silicon in silicon&#x2013;graphite composite electrodes. ACS Appl. Energy Mater. 5, 13367&#x2013;13376 (2022).\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#ref-CR69\" id=\"ref-link-section-d420863986e1299\" rel=\"nofollow noopener\" target=\"_blank\">69<\/a>,<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 70\" title=\"Kirkaldy, N., Samieian, M. A., Offer, G. J., Marinescu, M. &amp; Patel, Y. Lithium-ion battery degradation: comprehensive cycle ageing data and analysis for commercial 21700 cells. J. Power Sources 603, 234185 (2024).\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#ref-CR70\" id=\"ref-link-section-d420863986e1302\" rel=\"nofollow noopener\" target=\"_blank\">70<\/a>. The method used the low-rate 0.1\u2009C discharge curves, obtained from the RPT at BoL and after each degradation set, as a proxy for the full-cell OCV curve. A multi-parameter optimization function was then used to reconstruct this measured full-cell curve. The reconstruction was conducted by simulating a full-cell OCV curve from reference half-cell OCV curves for each electrode. These reference half-cell curves were sourced from literature<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 69\" title=\"Kirkaldy, N., Samieian, M. A., Offer, G. J., Marinescu, M. &amp; Patel, Y. Lithium-ion battery degradation: measuring rapid loss of active silicon in silicon&#x2013;graphite composite electrodes. ACS Appl. Energy Mater. 5, 13367&#x2013;13376 (2022).\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#ref-CR69\" id=\"ref-link-section-d420863986e1306\" rel=\"nofollow noopener\" target=\"_blank\">69<\/a>,<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 70\" title=\"Kirkaldy, N., Samieian, M. A., Offer, G. J., Marinescu, M. &amp; Patel, Y. Lithium-ion battery degradation: comprehensive cycle ageing data and analysis for commercial 21700 cells. J. Power Sources 603, 234185 (2024).\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#ref-CR70\" id=\"ref-link-section-d420863986e1309\" rel=\"nofollow noopener\" target=\"_blank\">70<\/a>. The optimization function minimized the error between the measured and simulated OCV curves by adjusting key parameters: the upper and lower lithiation limits of each electrode, and the relative capacity fraction of graphite and silicon in the composite anode. By tracking the changes in these fitted parameters relative to their BoL values, the total capacity loss was converted into LLI, LAMPE and LAMNE at each stage of degradation.<\/p>\n<p>Thermal abuse failure measurements<\/p>\n<p>To validate our TR failure submodel, thermal abuse failure tests were conducted using an abuse oven under various temperatures as well as an extended-volume accelerating rate calorimetry (ARC) manufactured by Thermal Hazard Technology with an adiabatic boundary surrounding cells. The experimental setups are shown in Supplementary Fig. <a data-track=\"click\" data-track-label=\"link\" data-track-action=\"supplementary material anchor\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#MOESM1\" rel=\"nofollow noopener\" target=\"_blank\">5<\/a>. During the oven tests, a custom-made mica block was used to hold the test cell with two K-type thermocouples attached to opposite central surfaces of the cell. The cell was initially placed in the oven chamber at room temperature, and the chamber was then heated with a constant dT\/dt of 4\u2009\u00b0C\u2009min\u22121. The extended-volume ARC setup included a 4-l canister at the center of its chamber to monitor gas generation, which was equipped with a pressure sensor to measure gas pressure. Inside the canister, four K-type thermocouples were placed, with three attached to the cell surface at constant intervals, and the fourth placed atop the cell venting valve to measure air temperature within the canister. An enhanced system accelerating rate calorimeter, manufactured by Thermal Hazard Technology, was used in the experiments for validating the states on the safety zone boundaries. The TR behaviors were tested using the \u2018Heat\u2013Wait\u2013Seek (HWS)\u2019 mode, with test parameters listed in Supplementary Table <a data-track=\"click\" data-track-label=\"link\" data-track-action=\"supplementary material anchor\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#MOESM1\" rel=\"nofollow noopener\" target=\"_blank\">2<\/a>. All cells were charged to 100% SoC using a 0.3\u2009C constant current\u2013constant voltage protocol, until the current dropped 0.01\u2009C, before the thermal abuse failure tests. Temperature signals during the oven tests and ARC tests were recorded at frequencies of 1\u2009Hz and 300\u2009Hz, respectively, and the pressure signals were recorded at 30-s intervals.<\/p>\n<p>Physics-based degradation-safety model development<\/p>\n<p>The physics-based degradation-safety model, which has enabled systematic analyses of degradation effects on battery safety, was developed by extending the degradation model we previously developed<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 32\" title=\"O&#x2019;Kane, S. E. J. et al. Lithium-ion battery degradation: how to model it. Phys. Chem. Chem. Phys. 24, 7909&#x2013;7922 (2022).\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#ref-CR32\" id=\"ref-link-section-d420863986e1343\" rel=\"nofollow noopener\" target=\"_blank\">32<\/a>,<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 33\" title=\"Li, R., O&#x2019;Kane, S., Marinescu, M. &amp; Offer, G. J. Modelling solvent consumption from SEI layer growth in lithium-ion batteries. J. Electrochem. Soc. 169, 060516 (2022).\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#ref-CR33\" id=\"ref-link-section-d420863986e1346\" rel=\"nofollow noopener\" target=\"_blank\">33<\/a> to couple with TR failure mechanisms. The degradation submodel is based on the classical Doyle\u2013Fuller\u2013Newman (DFN) model<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 71\" title=\"Doyle, M., Fuller, T. F. &amp; Newman, J. Modeling of galvanostatic charge and discharge of the lithium\/polymer\/insertion cell. J. Electrochem. Soc. 140, 1526&#x2013;1533 (1993).\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#ref-CR71\" id=\"ref-link-section-d420863986e1350\" rel=\"nofollow noopener\" target=\"_blank\">71<\/a> and includes strongly coupled models of SEI layer growth, electrolyte dry-out, Li plating, particle cracking and associated loss of active materials. The DFN model solves charge and mass conservation in the electrodes and electrolyte of a battery cell, with the total current density contributed by both Li (de)intercalation and degradation side reactions (for details see <a data-track=\"click\" data-track-label=\"link\" data-track-action=\"supplementary material anchor\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#MOESM1\" rel=\"nofollow noopener\" target=\"_blank\">Supplementary Methods<\/a>). The SEI layer growth process is modeled using the diffusion-limited SEI model<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 72\" title=\"Safari, M., Morcrette, M., Teyssot, A. &amp; Delacourt, C. Multimodal physics-based aging model for life prediction of Li-ion batteries. J. Electrochem. Soc. 156, A145&#x2013;A153 (2009).\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#ref-CR72\" id=\"ref-link-section-d420863986e1357\" rel=\"nofollow noopener\" target=\"_blank\">72<\/a>, which assumes that the thickness growth rate of an SEI layer is limited by the solvent transport through the outer SEI layer<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 73\" title=\"Single, F., Latz, A. &amp; Horstmann, B. Identifying the mechanism of continued growth of the solid&#x2013;electrolyte interphase. ChemSusChem 11, 1950&#x2013;1955 (2018).\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#ref-CR73\" id=\"ref-link-section-d420863986e1361\" rel=\"nofollow noopener\" target=\"_blank\">73<\/a><\/p>\n<p>$$\\frac{\\partial {L}_{\\mathrm{SEI}}}{\\partial t}=-\\frac{1}{2}{N}_{\\mathrm{sol}}\\overline{v}_{\\mathrm{SEI}},$$<\/p>\n<p>\n                    (1)\n                <\/p>\n<p>with the solvent flux, Nsol, described by<\/p>\n<p>$${N}_{\\mathrm{sol}}=-{D}_{\\mathrm{sol}}\\left(T\\right)\\frac{\\partial {c}_{\\mathrm{sol}}}{\\partial l},$$<\/p>\n<p>\n                    (2)\n                <\/p>\n<p>where \\(\\overline{v}_{\\mathrm{SEI}}\\) is SEI partial molar volume, csol is the solvent concentration, \\({D}_{\\text{sol}}\\left(T\\right)\\) is the temperature-dependent diffusivity and l represents the location along the SEI layer.<\/p>\n<p>The voltage drop associated with the SEI layer growth, \u03b7SEI, is determined by<\/p>\n<p>$${\\eta }_{{\\rm{SEI}}}={\\rho }_{{\\rm{SEI}}}{L}_{{\\rm{SEI}}}\\frac{{J}_{{\\rm{tot}}}}{{a}_{{\\rm{n}}}}$$<\/p>\n<p>\n                    (3)\n                <\/p>\n<p>where an is the specific surface area of the negative electrode, \u03c1SEI is the ohmic resistivity, LSEI is the SEI layer thickness and Jtot is the total current density.<\/p>\n<p>The solvent consumption resulting from the SEI layer growth is modeled following the approach in our previous work<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 33\" title=\"Li, R., O&#x2019;Kane, S., Marinescu, M. &amp; Offer, G. J. Modelling solvent consumption from SEI layer growth in lithium-ion batteries. J. Electrochem. Soc. 169, 060516 (2022).\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#ref-CR33\" id=\"ref-link-section-d420863986e1716\" rel=\"nofollow noopener\" target=\"_blank\">33<\/a>, wherein the amount of solvent consumed over a time interval \u0394t is calculated and incorporated into the DFN model. By assuming that the electrolyte reservoir is empty, the change of cell cross-sectional area Acell due to solvent consumption is calculated using equations (<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"equation anchor\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#Equ4\" rel=\"nofollow noopener\" target=\"_blank\">4<\/a>)\u2013(<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"equation anchor\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#Equ7\" rel=\"nofollow noopener\" target=\"_blank\">7<\/a>)<\/p>\n<p>$$\\Delta{n}_{\\mathrm{SEI}}=\\frac{{A}_{\\mathrm{cell}}(t)}{\\overline{v}_{\\mathrm{SEI}}}{\\int }_{0}^{{L}_{{\\rm{n}}}}{a}_{{\\mathrm{n}}}[{L}_{\\mathrm{SEI}}\\left(t+\\Delta{t}\\right)-{L}_{\\mathrm{SEI}}]{\\rm{d}}x,$$<\/p>\n<p>\n                    (4)\n                <\/p>\n<p>$${\\mathrm{Ratio}}_{\\mathrm{dry}}=\\frac{{V}_{{\\rm{e}}}\\left(t\\right)+\\Delta{n}_{\\mathrm{SEI}}(\\overline{v}_{\\mathrm{SEI}}-2\\overline{v}_{\\mathrm{EC}})}{{V}_{{\\rm{e}}}\\left(t\\right)},$$<\/p>\n<p>\n                    (5)\n                <\/p>\n<p>$${V}_{{\\rm{e}}}\\left(t\\right)={A}_{\\mathrm{cell}}\\left(t\\right)[{L}_{{\\mathrm{n}}}{\\varepsilon }_{{\\mathrm{n}}}\\left(t\\right)+{L}_{{\\mathrm{sep}}}{\\varepsilon }_{{\\mathrm{sep}}}+{L}_{{\\mathrm{p}}}{\\varepsilon }_{{\\mathrm{p}}}],$$<\/p>\n<p>\n                    (6)\n                <\/p>\n<p>$${A}_{\\mathrm{cell}}\\left(t+\\Delta{t}\\right)={\\mathrm{Ratio}}_{\\mathrm{dry}}{A}_{\\mathrm{cell}}\\left(t\\right),$$<\/p>\n<p>\n                    (7)\n                <\/p>\n<p>where \u0394nSEI is the amount change of SEI, \\(\\overline{v}_{\\mathrm{EC}}\\) is the partial molar volume for the solvent of ethylene carbonate, Ln is the negative electrode thickness, x is the spatial coordinate along the negative electrode thickness, Ratiodry denotes the shrinking ratio of the cross-sectional area, Ve is the electrolyte volume, \u03b5n is the negative electrode porosity, Lsep is the separator thickness, \u03b5sep is the separator porosity, Lp is the positive electrode thickness and \u03b5p is the positive electrode porosity.<\/p>\n<p>Li formation, stripping and the subsequent decay of plated Li into dead Li are simulated using a partially reversible Li plating model, where the concentration change of plated Li is correlated with the Li plating current density, JLi; the Faraday constant, F; and the rate of conversion of plated Li to \u2018dead Li\u2019, \u03b3LicLi, (ref. <a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 32\" title=\"O&#x2019;Kane, S. E. J. et al. Lithium-ion battery degradation: how to model it. Phys. Chem. Chem. Phys. 24, 7909&#x2013;7922 (2022).\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#ref-CR32\" id=\"ref-link-section-d420863986e2585\" rel=\"nofollow noopener\" target=\"_blank\">32<\/a>) by<\/p>\n<p>$$\\frac{\\partial {c}_{\\mathrm{Li}}}{\\partial t}=\\frac{-{J}_{\\text{Li}}}{F}-{\\gamma }_{\\mathrm{Li}}{c}_{\\mathrm{Li}},$$<\/p>\n<p>\n                    (8)\n                <\/p>\n<p>with the Li plating current density determined from the Butler\u2013Volmer equation, and the decay rate to \u2018dead Li\u2019, \u03b3Li, assumed to be diffusion limited and dependent on the SEI thickness by<\/p>\n<p>$$\\gamma ={\\gamma }_{0}\\frac{{L}_{\\mathrm{SEI},0}}{{L}_{\\mathrm{SEI}}},$$<\/p>\n<p>\n                    (9)\n                <\/p>\n<p>The porosity change due to SEI layer growth and partially reversible Li plating is determined by<\/p>\n<p>$$\\frac{{\\rm{d}}\\varepsilon }{{\\rm{d}}t}=-{a}_{{\\mathrm{n}}}\\ \\frac{{\\rm{d}}{L}_{\\mathrm{tot}}}{{\\rm{d}}t},$$<\/p>\n<p>\n                    (10)\n                <\/p>\n<p>where Ltot is the total thickness of deposition calculated as<\/p>\n<p>$${L}_{\\mathrm{tot}}={L}_{\\mathrm{SEI}}+{c}_{\\mathrm{Li}}\\frac{{\\overline{v}}_{\\mathrm{Li}}}{{a}_{{\\mathrm{n}}}}+{c}_{\\mathrm{dl}}\\frac{{\\overline{v}}_{\\mathrm{Li}}}{{a}_{{\\mathrm{n}}}},$$<\/p>\n<p>\n                    (11)\n                <\/p>\n<p>where cLi and cdl denote the concentrations of active plated Li and dead Li, respectively.<\/p>\n<p>Electrode particle fracture and crack propagation are unified into a single stress-based model<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 74\" title=\"Zhang, X., Shyy, W. &amp; Sastry, A. M. Numerical simulation of intercalation-induced stress in Li-ion battery electrode particles. J. Electrochem. Soc. 154, A910 (2007).\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#ref-CR74\" id=\"ref-link-section-d420863986e3112\" rel=\"nofollow noopener\" target=\"_blank\">74<\/a>, with the radial stress \u03c3r and tangential stress \u03c3t solved by<\/p>\n<p>$${\\sigma }_{{\\rm{r}}}=\\frac{2\\varOmega \\psi }{\\left(1-\\nu \\right)}\\left[{c}_{{\\rm{avg}}}\\left({R}_{i}\\right)-{c}_{{\\rm{avg}}}\\left(r\\right)\\right]$$<\/p>\n<p>\n                    (12)\n                <\/p>\n<p>$${\\sigma }_{{\\rm{t}}}=\\frac{\\Omega \\psi }{\\left(1-\\nu \\right)}\\left[2{c}_{\\mathrm{avg}}\\left({R}_{i}\\right)+{c}_{\\mathrm{avg}}\\left(r\\right)-\\overline{c}\/3\\right)],$$<\/p>\n<p>\n                    (13)\n                <\/p>\n<p>where \u03a9 denotes the partial molar volume, \u03c8 is the Young\u2019s modulus, \u03bd is the Poisson\u2019s ratio, R denotes the radius of the particle, \\({c}_{\\text{avg}}\\left(r\\right)\\) is the average Li-ion concentration and \\(\\bar{c}\\) is the difference between the Li concentration and reference value.<\/p>\n<p>The fatigue crack growth is solved by Paris\u2019 law as below<\/p>\n<p>$$\\frac{{\\rm{d}}{l}_{\\mathrm{cr}}}{{\\rm{d}}N}=\\frac{{k}_{\\mathrm{cr}}}{{t}_{0}}{\\left({\\sigma }_{{\\rm{t}}}{b}_{\\mathrm{cr}}\\sqrt{{\\uppi }{l}_{\\mathrm{cr}}}\\right)}^{{\\lambda }_{\\mathrm{cr}}},{\\mathrm{when}}\\;{\\sigma }_{{\\rm{t}}} &gt; 0,$$<\/p>\n<p>\n                    (14)\n                <\/p>\n<p>where t0 is the cycle number, kcr is the correction factor for stress intensity, and bcr and \u03bbcr are constants.<\/p>\n<p>The loss of active material (LAM) due to stress is calculated by<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 32\" title=\"O&#x2019;Kane, S. E. J. et al. Lithium-ion battery degradation: how to model it. Phys. Chem. Chem. Phys. 24, 7909&#x2013;7922 (2022).\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#ref-CR32\" id=\"ref-link-section-d420863986e3671\" rel=\"nofollow noopener\" target=\"_blank\">32<\/a><\/p>\n<p>$$\\frac{\\partial {\\varepsilon }_{{\\rm{s}},k}}{\\partial t}=\\frac{\\beta }{{t}_{0}}{\\left(\\frac{{\\sigma }_{{\\rm{h}}}}{{\\sigma }_{{\\rm{c}}}}\\right)}^{{\\lambda }_{\\mathrm{LAM}}},\\,\\mathrm{when}\\,{\\sigma }_{{\\rm{h}}} &gt; 0,$$<\/p>\n<p>\n                    (15)\n                <\/p>\n<p>$${\\sigma }_{{\\rm{h}}}=\\left({\\sigma }_{{\\rm{r}}}+2{\\sigma }_{{\\rm{t}}}\\right)\/3,$$<\/p>\n<p>\n                    (16)\n                <\/p>\n<p>where \u03b5a,k is the volume fraction for active materials, \u03b2 and \u03bbLAM are constants of LAM proportional and exponential terms, and \u03c3c is the critical stress.<\/p>\n<p>The TR failure submodel considers thermal decomposition reactions and their associated heat and gas generation, pressure buildup and vent flow dynamics. The energy conservation equation during TR is as follows<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 75\" title=\"He, C. X., Yue, Q. L., Chen, Q. &amp; Zhao, T. S. Modeling thermal runaway of lithium-ion batteries with a venting process. Appl. Energy 327, 120110 (2022).\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#ref-CR75\" id=\"ref-link-section-d420863986e3871\" rel=\"nofollow noopener\" target=\"_blank\">75<\/a>:<\/p>\n<p>$${m}_{\\mathrm{cell}}{\\mathrm{Cp}}_{\\mathrm{cell}}\\frac{{\\rm{d}}{T}_{\\mathrm{cell}}}{{\\rm{d}}t}=\\sum {\\dot{Q}}_{i}+{\\dot{Q}}_{\\mathrm{diss}}+{\\dot{Q}}_{\\mathrm{ISC}}+{\\dot{Q}}_{\\mathrm{evap}}+{\\dot{m}}_{\\mathrm{vent}}\\Delta{H}_{\\mathrm{vent}},$$<\/p>\n<p>\n                    (17)\n                <\/p>\n<p>where \\({\\dot{Q}}_{i}\\), \\({\\dot{Q}}_{{\\rm{diss}}}\\), \\({\\dot{Q}}_{{\\rm{ISC}}}\\), \\({\\dot{Q}}_{{\\rm{evap}}}\\) and \\({\\dot{m}}_{{\\rm{vent}}}{h}_{{\\rm{vent}}}\\) represent heat generation rate from the reaction i, heat dissipation rate, heat generation from ISC, evaporation heat from solvents and energy loss to ejecta, respectively. The reaction heat generation rate is determined by<\/p>\n<p>$${\\dot{Q}}_{i}\\left(t\\right)={m}_{i}\\Delta{H}_{i}\\frac{{\\rm{d}}{c}_{i}^{* }\\left(t\\right)}{{\\rm{d}}t},$$<\/p>\n<p>\n                    (18)\n                <\/p>\n<p>with the reaction rate calculated by the Arrhenius law<\/p>\n<p>$$\\frac{{\\rm{d}}{c}_{i}^{* }\\left(t\\right)}{{\\rm{d}}t}={B}_{i}\\exp \\left(-\\frac{{E}_{i}}{R{T}_{\\mathrm{cell}}\\left(t\\right)}\\right){f}_{i}\\left({c}_{i}^{* }\\left(t\\right)\\right),$$<\/p>\n<p>\n                    (19)\n                <\/p>\n<p>where R denotes the gas constant and Bi, \\({c}_{i}^{* }\\left(t\\right)\\) and Ei denote the frequency, normalized reactant concentration and activation energy of the reaction i, which connect to the degradation submodel. \\({f}_{i}\\left({c}_{i}^{* }\\left(t\\right)\\right)\\) is a modification factor, varying for different reactions and linking back to the degradation submodel.<\/p>\n<p>The calculation of the internal pressure within the battery before venting follows Dalton\u2019s law, accounting for contributions from both generated gases and electrolyte vapor<\/p>\n<p>$${P}_{\\mathrm{tot}}={P}_{\\mathrm{gas}}+{P}_{\\mathrm{elec}},$$<\/p>\n<p>\n                    (20)\n                <\/p>\n<p>with the partial pressures of generated gases, Pgas, derived from the ideal gas law alongside kinetics of gas-generating reactions, and the electrolyte vapor pressure determined as the saturated pressure using Antoine\u2019s equation<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 76\" title=\"Zhang, X., Zuo, J. &amp; Jian, C. Experimental isobaric vapor-liquid equilibrium for binary systems of ethyl methyl carbonate + methanol, + ethanol, + dimethyl carbonate, or + diethyl carbonate at 101.3&#x2009;kPa. J. Chem. Eng. Data 55, 4896&#x2013;4902 (2010).\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#ref-CR76\" id=\"ref-link-section-d420863986e4746\" rel=\"nofollow noopener\" target=\"_blank\">76<\/a>. At each time step, the total internal pressure is compared with the vent pressure (2\u2009MPa for LG M50T cells). If it is lower than the vent pressure, the partial pressures calculations are repeated. If the pressure exceeds the vent pressure, the vent valve opens, and the dynamics of vent flow are calculated as an isentropic nozzle flow, considering two flow conditions: subsonic flow and chocked flow as determined by the inequality<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 77\" title=\"Kong, D., Wang, G., Ping, P. &amp; Wen, J. A coupled conjugate heat transfer and CFD model for the thermal runaway evolution and jet fire of 18650 lithium-ion battery under thermal abuse. eTransportation 12, 100157 (2022).\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#ref-CR77\" id=\"ref-link-section-d420863986e4750\" rel=\"nofollow noopener\" target=\"_blank\">77<\/a><\/p>\n<p>$$\\frac{{P}_{\\mathrm{amb}}}{{P}_{\\mathrm{cell}}} &gt; {\\left(\\frac{2}{\\theta +1}\\right)}^{\\frac{\\theta }{\\theta -1}},$$<\/p>\n<p>\n                    (21)\n                <\/p>\n<p>where \u03b8 is the heat capacity ratio of venting gases. The flow dynamics calculations yield the vent gas velocity, facilitating the calculation of the vent mass flow rate. The mass flow rate is subsequently substituted back into equation (<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"equation anchor\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#Equ17\" rel=\"nofollow noopener\" target=\"_blank\">17<\/a>) to calculate the heat carried by the vent mass and thus update the cell temperature. The degradation submodel is implemented in the open-source package Python Battery Mathematical Modelling (PyBaMM)<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 78\" title=\"Sulzer, V., Marquis, S. G., Timms, R., Robinson, M. &amp; Chapman, S. J. Python battery mathematical modelling (PyBaMM). J. Open Res. Softw. 9, 14 (2021).\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#ref-CR78\" id=\"ref-link-section-d420863986e4833\" rel=\"nofollow noopener\" target=\"_blank\">78<\/a> version 23.5, and the TR failure submodel is coded in Python and coupled with the PyBaMM degradation model. The flowchart of solving the model is shown in Extended Data Fig. <a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#Fig7\" rel=\"nofollow noopener\" target=\"_blank\">1<\/a>. Most model parameters were based on the PyBaMM parameter sets \u2018Okane2022\u2019 and \u2018Chen2020\u2019, which were obtained for LG M50T cylindrical cells through independent parameterization experiments<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 39\" title=\"O&#x2019;Regan, K., Brosa Planella, F., Widanage, W. D. &amp; Kendrick, E. Thermal-electrochemical parameters of a high energy lithium-ion cylindrical battery. Electrochim. Acta 425, 140700 (2022).\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#ref-CR39\" id=\"ref-link-section-d420863986e4840\" rel=\"nofollow noopener\" target=\"_blank\">39<\/a>,<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 40\" title=\"Chen, C.-H. et al. Development of experimental techniques for parameterization of multi-scale lithium-ion battery models. J. Electrochem. Soc. 167, 080534 (2020).\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#ref-CR40\" id=\"ref-link-section-d420863986e4843\" rel=\"nofollow noopener\" target=\"_blank\">40<\/a>. For model parameters not available in these data sets, their values were assumed on the basis of values reported in literature<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 32\" title=\"O&#x2019;Kane, S. E. J. et al. Lithium-ion battery degradation: how to model it. Phys. Chem. Chem. Phys. 24, 7909&#x2013;7922 (2022).\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#ref-CR32\" id=\"ref-link-section-d420863986e4847\" rel=\"nofollow noopener\" target=\"_blank\">32<\/a>. A full list of the model assumptions, equations, boundary conditions and input parameters is provided in <a data-track=\"click\" data-track-label=\"link\" data-track-action=\"supplementary material anchor\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#MOESM1\" rel=\"nofollow noopener\" target=\"_blank\">Supplementary Methods<\/a> and Supplementary Note <a data-track=\"click\" data-track-label=\"link\" data-track-action=\"supplementary material anchor\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#MOESM1\" rel=\"nofollow noopener\" target=\"_blank\">1<\/a>.<\/p>\n<p>Physics-based degradation-safety model validation<\/p>\n<p>A staged validation strategy, as depicted in Extended Data Fig. <a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#Fig7\" rel=\"nofollow noopener\" target=\"_blank\">1<\/a>, was adopted to evaluate the predictive fidelity of our model: first, the degradation and TR failure submodels were validated independently by comparing simulation results with degradation and thermal abuse tests; second, the integrated degradation-safety model was validated by comparing its predictions of safety zone and boundary evolutions under different degradation paths with experimental measurements. Owing to complex and competing interactions among degradation mechanisms, as demonstrated in our model parameter sensitivity analyses (Supplementary Note <a data-track=\"click\" data-track-label=\"link\" data-track-action=\"supplementary material anchor\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#MOESM1\" rel=\"nofollow noopener\" target=\"_blank\">2<\/a>), different combinations of degradation mechanisms may produce similar capacity trends. To ensure a proper assessment of the model\u2019s capability of capturing the underlying physics, the degradation submodel was validated not only against capacity retention data but also against voltage profiles and DM analysis results under different conditions designed to trigger different contributions from different degradation mechanisms. As shown in Extended Data Fig. <a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#Fig8\" rel=\"nofollow noopener\" target=\"_blank\">2<\/a>, the simulated capacity fade curves closely match the measurements, with a maximum mean percentage error (MPE) of 1.36%. Simulated terminal voltage profiles in different RPTs also show strong agreement with the experimental data, with a maximum MPE of 2.25%. Extended Data Fig. <a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#Fig9\" rel=\"nofollow noopener\" target=\"_blank\">3<\/a> further confirms the consistency between simulated and experimentally derived SoHs and DMs including LLI, LAMNE and LAMPE across all cycling conditions, with a maximum total MPE of 16.3% calculated using a weighted approach<\/p>\n<p>$$\\begin{array}{l}{\\mathrm{MPE}}_{\\mathrm{DM},\\mathrm{total}}=0.5{\\mathrm{MPE}}_{\\mathrm{SOH}}+0.3{\\mathrm{MPE}}_{\\mathrm{LLI}}+\\\\0.1{\\mathrm{MPE}}_{\\mathrm{LAMPE}}+0.1{\\mathrm{MPE}}_{\\mathrm{LAMNE}}.\\end{array}$$<\/p>\n<p>\n                    (22)\n                <\/p>\n<p>The weighting assigns a higher contribution (0.5) to SoH versus LLI (0.3) and LAMs (0.1) to reflect the higher confidence in the direct experimental measurements compared with the OCV-fitted values. This relatively higher MPE is mainly contributed by MPELAMNE under lower temperatures (10\u2009\u00b0C and 25\u2009\u00b0C) possibly owing to the limitation of our Paris\u2019 law-based cracking model in capturing anisotropic, diffusion-driven cracking in graphite particles. For the TR failure submodel, our sensitivity analyses revealed high sensitivity to the kinetic parameters governing the reaction rates of cathode decomposition, SEI decomposition and intercalated Li\u2013electrolyte reactions. Given the exponential temperature dependence of these reactions and the influence of thermal boundary conditions on heat transfer and temperature evolution, validation of the TR failure submodel was conducted using thermal abuse experiments under varied thermal boundary conditions. Extended Data Fig. <a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#Fig10\" rel=\"nofollow noopener\" target=\"_blank\">4<\/a> shows that the model successfully reproduces temperature and dT\/dt profiles in oven tests at different temperatures, with maximum MPEs of 1.25% and 7.85% for the venting and maximum temperatures. It also performs well in HWS ARC tests under adiabatic conditions. The integration of the two submodels was finally validated by comparing simulated and experimental path-dependent safety zones and boundaries over the battery cycle life. Two representative degradation paths were selected for the validation: 0.7\u2009C\/1\u2009C at 10\u2009\u00b0C (case 1), which leads to a downward shift in the safety boundary, and 0.3\u2009C\/1\u2009C at 40\u2009\u00b0C (case 3), which causes an upward shift. Owing to the extreme time requirements for experimentally measuring full safety zones and boundaries, two critical timepoints were measured for each selected degradation path: the BoL and the 3rd RPT (after the predicted turning point on the safety boundaries). Measurements were repeated under a baseline condition of 0.3\u2009C\/1\u2009C at 25\u2009\u00b0C, with an additional measurement at the EoL after 1,170 cycles. As shown in Extended Data Fig. <a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#Fig11\" rel=\"nofollow noopener\" target=\"_blank\">5<\/a>, the model results well capture the experimentally measured path-dependent evolution of different safety zone boundaries, except for some discrepancies in the near-TR boundaries in certain cases, possibly owing to the omission of gas crosstalk in our model, which has been demonstrated to affect cathode decomposition dominating the near-TR boundaries<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 61\" title=\"Wang, Y. et al. Reductive gas manipulation at early self-heating stage enables controllable battery thermal failure. Joule 6, 2810&#x2013;2820 (2022).\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#ref-CR61\" id=\"ref-link-section-d420863986e5023\" rel=\"nofollow noopener\" target=\"_blank\">61<\/a>. In summary, the validation strategy, designed as the minimal set of experiments for thoroughness, demonstrates the reliability of our model in capturing long-term degradation mechanisms and performance, TR failure behaviors and coupled degradation-safety dynamics of lithium-ion batteries. Details of experimental repeatability are provided in Supplementary Note <a data-track=\"click\" data-track-label=\"link\" data-track-action=\"supplementary material anchor\" href=\"http:\/\/www.nature.com\/articles\/s44286-026-00465-1#MOESM1\" rel=\"nofollow noopener\" target=\"_blank\">3<\/a>.<\/p>\n","protected":false},"excerpt":{"rendered":"Degradation measurements To prepare degraded cells for thermal abuse failure experiments and validate our degradation submodel, degradation measurements&hellip;\n","protected":false},"author":2,"featured_media":794794,"comment_status":"","ping_status":"","sticky":false,"template":"","format":"standard","meta":{"footnotes":"","_share_on_mastodon":"0"},"categories":[74],"tags":[58265,8406,8409,18,9656,330842,910,19,330841,17,283460,82,330843],"class_list":["post-794793","post","type-post","status-publish","format-standard","has-post-thumbnail","category-technology","tag-batteries","tag-chemical-engineering","tag-chemistry-food-science","tag-eire","tag-engineering","tag-environmental-engineering-biotechnology","tag-general","tag-ie","tag-industrial-chemistry-chemical-engineering","tag-ireland","tag-materials-engineering","tag-technology","tag-theoretical-and-computational-chemistry"],"share_on_mastodon":{"url":"https:\/\/pubeurope.com\/@ie\/117665909367013710","error":""},"_links":{"self":[{"href":"https:\/\/www.europesays.com\/ie\/wp-json\/wp\/v2\/posts\/794793","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/www.europesays.com\/ie\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/www.europesays.com\/ie\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/www.europesays.com\/ie\/wp-json\/wp\/v2\/users\/2"}],"replies":[{"embeddable":true,"href":"https:\/\/www.europesays.com\/ie\/wp-json\/wp\/v2\/comments?post=794793"}],"version-history":[{"count":0,"href":"https:\/\/www.europesays.com\/ie\/wp-json\/wp\/v2\/posts\/794793\/revisions"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/www.europesays.com\/ie\/wp-json\/wp\/v2\/media\/794794"}],"wp:attachment":[{"href":"https:\/\/www.europesays.com\/ie\/wp-json\/wp\/v2\/media?parent=794793"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/www.europesays.com\/ie\/wp-json\/wp\/v2\/categories?post=794793"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/www.europesays.com\/ie\/wp-json\/wp\/v2\/tags?post=794793"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}