{"id":796518,"date":"2026-11-24T16:17:28","date_gmt":"2026-11-24T16:17:28","guid":{"rendered":"https:\/\/www.europesays.com\/ie\/796518\/"},"modified":"2026-11-24T16:17:28","modified_gmt":"2026-11-24T16:17:28","slug":"highly-reinforced-self-cleaning-low-density-polyethylene-polyvinyl-butyral-bismuth-oxide-nanocomposites-fabricated-by-electron-beam-irradiation","status":"publish","type":"post","link":"https:\/\/www.europesays.com\/ie\/796518\/","title":{"rendered":"Highly reinforced self-cleaning low-density polyethylene\/poly(vinyl butyral)\/bismuth oxide nanocomposites fabricated by electron beam irradiation"},"content":{"rendered":"<p>Characterization of Bi2O3 nanoparticles<\/p>\n<p>Figure <a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig1\" rel=\"nofollow noopener\" target=\"_blank\">1<\/a>a presents the TEM micrograph of Bi2O3 nanoparticles, revealing the formation of a dark, spherical, and uniformly distributed morphology with an average diameter ranging from 2 to 21\u00a0nm. Additionally, the TEM image indicates that most particles are well dispersed with limited agglomeration, which can be attributed to the high surface energy and nanoscale nature of the particles. The homogeneous distribution and small particle size are advantageous for enhancing the interfacial interaction between Bi2O3 nanoparticles and the polymer matrix in nanocomposite applications.<\/p>\n<p>The XRD pattern of Bi2O3 nanoparticles (Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig1\" rel=\"nofollow noopener\" target=\"_blank\">1<\/a>b) reveals a well-crystallized monoclinic \u03b1-phase structure, consistent with JCPDS card No. 41-1449. The diffractogram exhibits a series of distinct and sharp diffraction peaks, confirming the high crystallinity of the synthesized nanoparticles. The two most intense peaks appear at 2\u03b8\u2009=\u200927.44\u00b0 and 28.06\u00b0, corresponding to the (002) and (200) crystallographic planes, respectively, which are the characteristic signature reflections of the monoclinic Bi2O3 phase.<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 37\" title=\"Wahba, M. A., Yakout, S. M., Abdel-Monem, Y. K. &amp; Hammood, A. A. A. Simple and easy control-synthesis of pure &#x3B1;-Bi2O3 and Bi2O2CO3: Morphological, optical and solar photon-energy photocatalytic studies. Chem. Afr. 7, 195&#x2013;207 (2024).\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#ref-CR37\" id=\"ref-link-section-d3355104e904\" rel=\"nofollow noopener\" target=\"_blank\">37<\/a>,<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 38\" title=\"Malligavathy, M. &amp; Pathinettam Padiyan, D. Role of pH in the hydrothermal synthesis of phase pure alpha Bi2O3 nanoparticles and its structural characterization. Adv. Mater. Proc. 2, 51&#x2013;55 (2017).\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#ref-CR38\" id=\"ref-link-section-d3355104e907\" rel=\"nofollow noopener\" target=\"_blank\">38<\/a>. Additional peaks are observed at 2\u03b8\u2009=\u200923.97\u00b0 (120), 25.91\u00b0 (021), 31.77\u00b0 (121), 32.69\u00b0 (220), 33.30\u00b0 (012), 35.07\u00b0 (211), 36.26\u00b0 (022), 39.46\u00b0 (122), 41.13\u00b0 (300), 46.34\u00b0 (222), 47.21\u00b0 (040), 52.45\u00b0 (141), 55.79\u00b0 (004), 57.83\u00b0 (321), and 64.12\u00b0 (421). The sharp and intense diffraction peaks confirm the crystalline nature and high purity of the synthesized Bi2O3 nanoparticles.<\/p>\n<p><b id=\"Fig1\" class=\"c-article-section__figure-caption\" data-test=\"figure-caption-text\">Fig. 1<\/b><img decoding=\"async\" aria-describedby=\"figure-1-desc\" src=\"https:\/\/www.europesays.com\/ie\/wp-content\/uploads\/2026\/11\/41598_2026_75938_Fig1_HTML.png\" alt=\"Fig. 1\" loading=\"lazy\" width=\"685\" height=\"847\"\/><\/p>\n<p>(<b>a<\/b>) TEM micrograph and (<b>b<\/b>) XRD pattern of Bi2O3 nanoparticles.<\/p>\n<p>Mechanical properties of LDPE\/PVB blend<\/p>\n<p>Figure <a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig2\" rel=\"nofollow noopener\" target=\"_blank\">2<\/a> illustrates the effect of PVB ratio (3, 5, and 10%) on the mechanical properties of LDPE\/PVB blends, including tensile strength, elongation at break, and elastic modulus. It is known that the mechanical properties of a blend of two polymers depend mainly on the compatibility between the two polymers, blend ratio, and any compatibilizers used during processing. It is known that LDPE is flexible, ductile, chemically resistant, and has good elongation at break, but relatively low strength and stiffness. On the other hand, PVB is flexible, adhesive, tough, and has excellent impact resistance.<\/p>\n<p>The tensile strength (Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig2\" rel=\"nofollow noopener\" target=\"_blank\">2<\/a>a) increased from 13.3\u00a0MPa for neat LDPE to 14.8\u00a0MPa and 15.5\u00a0MPa for blends containing 3 and 5 wt% PVB, respectively. This improvement indicates enhanced stress transfer and favorable interfacial interactions between LDPE and the dispersed PVB phase. However, when the PVB content was increased to 10 wt%, the tensile strength decreased to about 13.9\u00a0MPa, suggesting that excessive PVB loading may lead to phase separation or the formation of stress concentration sites, which negatively affect the mechanical performance of the blend. The elongation at break (Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig2\" rel=\"nofollow noopener\" target=\"_blank\">2<\/a>b) showed a continuous decrease with increasing PVB content. Neat LDPE exhibited a high elongation at break of 860%, reflecting its highly ductile nature. The elongation decreased to about 780%, 620%, and 600% for blends containing 3, 5, and 10 wt% PVB, respectively. This reduction indicates that the incorporation of PVB into LDPE texture enhances the stiffness of the polymeric matrix and hence decreases the elongation percent<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 39\" title=\"Bekhit, M., Fathy, E. S. &amp; Sharaf, A. Effect of gamma irradiation on properties of the synthesized PANI-Cu nanoparticles assimilated into PS polymer for electromagnetic interference shielding application. Sci. Rep. 14, 16403 (2024).\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#ref-CR39\" id=\"ref-link-section-d3355104e965\" rel=\"nofollow noopener\" target=\"_blank\">39<\/a>. A similar trend was observed for the elastic modulus (Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig2\" rel=\"nofollow noopener\" target=\"_blank\">2<\/a>c) as in tensile strength. The elastic modulus increased from 9.6\u00a0MPa for neat LDPE to 10.4\u00a0MPa and reached a maximum value of 10.8\u00a0MPa at 5 wt% PVB, demonstrating an increase in stiffness due to the reinforcing effect of PVB. However, further increasing the PVB content to 10 wt% caused a significant decrease in elastic modulus to 6.7\u00a0MPa, which may be attributed to reduced blend homogeneity and weaker interfacial interaction at higher PVB concentrations. Based on the results, the incorporation of 5 wt% PVB provides the optimum balance between strength and stiffness while maintaining reasonable ductility. The enhancement in tensile strength and elastic modulus at low PVB contents confirms the effectiveness of PVB as a reinforcing component in LDPE. The results indicated that the optimum LDPE\/PVB blend ratio was 95\/5 wt%.<\/p>\n<p><b id=\"Fig2\" class=\"c-article-section__figure-caption\" data-test=\"figure-caption-text\">Fig. 2<\/b><img decoding=\"async\" aria-describedby=\"figure-2-desc\" src=\"https:\/\/www.europesays.com\/ie\/wp-content\/uploads\/2026\/11\/41598_2026_75938_Fig2_HTML.png\" alt=\"Fig. 2\" loading=\"lazy\" width=\"685\" height=\"517\"\/><\/p>\n<p>Mechanical properties of LDPE\/PVB blends containing different PVB contents; (<b>a<\/b>) tensile strength, (<b>b<\/b>) elongation at break (%), and (<b>c<\/b>) elastic modulus.<\/p>\n<p>Effect of EB irradiation on the mechanical properties of LDPE\/PVB\/Bi2O3 nanocomposites<\/p>\n<p>Figure <a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig3\" rel=\"nofollow noopener\" target=\"_blank\">3<\/a> presents the effect of electron-beam irradiation dose on the mechanical properties (tensile strength, elongation at break, and elastic modulus) of LDPE\/5%PVB loaded with a fixed ratio of 3 phr Bi2O3 nanocomposites. LDPE is a nonpolar polymer, whereas PVB contains polar hydroxyl groups; consequently, LDPE\/PVB blends are generally characterized by limited compatibility and partial immiscibility. The poor interfacial interaction between the two polymer phases can adversely affect the mechanical properties of the blend. Therefore, EB irradiation was employed at doses of 10, 30, 50, 100, 120, and 150\u00a0kGy to enhance interfacial interactions and improve the compatibilization between the LDPE and PVB matrices through radiation-induced crosslinking. As shown in Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig3\" rel=\"nofollow noopener\" target=\"_blank\">3<\/a>a, the tensile strength of LDPE\/PVB\/Bi2O3 nanocomposites increased progressively with rising EB irradiation dose. It rose from 13.3\u00a0MPa for the unirradiated sample to 14.3, 14.7, and 15.4\u00a0MPa at 10, 30, and 50\u00a0kGy, respectively. A pronounced enhancement was observed at higher doses (100\u2013120\u00a0kGy), reaching 17.0\u00a0MPa, whereas at 150\u00a0kGy a slight decrease was predominant.<\/p>\n<p>This enhancement is attributed to radiation-induced crosslinking within the polymer matrix, which strengthens the interfacial interactions among LDPE, PVB, and Bi\u2082O\u2083 nanoparticles. The elongation at break (Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig3\" rel=\"nofollow noopener\" target=\"_blank\">3<\/a>b) also exhibited a remarkable increase with rising irradiation dose, reaching its maximum at 100\u00a0kGy. The observed increase in elongation in the presence of Bi\u2082O\u2083 may be linked to the strain-induced crystallization effect commonly reported in polymer composites<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 39\" title=\"Bekhit, M., Fathy, E. S. &amp; Sharaf, A. Effect of gamma irradiation on properties of the synthesized PANI-Cu nanoparticles assimilated into PS polymer for electromagnetic interference shielding application. Sci. Rep. 14, 16403 (2024).\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#ref-CR39\" id=\"ref-link-section-d3355104e1035\" rel=\"nofollow noopener\" target=\"_blank\">39<\/a>,<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 40\" title=\"Hassan, M. M., Aly, R. O., Aal, S. E. A., El-Masry, A. M. &amp; Fathy, E. S. Styrene butadiene-based blends containing waste rubber powder: Physico-mechanical effects of mechanochemical devulcanization and gamma irradiation. J. Ind. Eng. Chem. 19, 1735&#x2013;1742 (2013).\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#ref-CR40\" id=\"ref-link-section-d3355104e1038\" rel=\"nofollow noopener\" target=\"_blank\">40<\/a>. At higher doses (120\u2013150\u00a0kGy), however, the elongation declined, reflecting the increased stiffness and restricted chain mobility within the polymer matrix.<\/p>\n<p>The elastic modulus (Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig3\" rel=\"nofollow noopener\" target=\"_blank\">3<\/a>c) of LDPE\/PVB\/Bi2O3 nanocomposites increased steadily with rising electron-beam irradiation dose. It rose from 9.6\u00a0MPa for the unirradiated sample to 10.0, 10.6, and 10.8\u00a0MPa at 10, 30, and 50\u00a0kGy, respectively. A further enhancement was observed at higher doses, reaching 11.3\u00a0MPa at 100\u00a0kGy, followed by slight increments at 120\u2013150\u00a0kGy, indicating a gradual approach toward saturation in stiffness improvement. EB irradiation effectively enhanced the mechanical properties of the LDPE\/PVB\/Bi2O3 nanocomposite by improving crosslinking and interfacial compatibility within the polymer matrix. Among the studied doses, 100\u00a0kGy yielded the best overall mechanical performance, indicating the most favorable balance between network formation and structural stability. The results are consistent with previous reports on LDPE\/carbon black nanocomposites; moreover, EB irradiation at 100\u00a0kGy was shown to yield optimal mechanical performance and increased crosslinking, supporting the interpretation that irradiation effectively modifies the polymer network and surface morphology.<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 41\" title=\"Akhavan, A., Khoylou, F., Sheikh, N. &amp; Kazeminejad, H. Effect of electron beam irradiation on the thermal, mechanical and aging behaviors of polyethylene\/carbon black nanocomposite. Radiat. Phys. Chem. 187, 109582 (2021).\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#ref-CR41\" id=\"ref-link-section-d3355104e1057\" rel=\"nofollow noopener\" target=\"_blank\">41<\/a><\/p>\n<p><b id=\"Fig3\" class=\"c-article-section__figure-caption\" data-test=\"figure-caption-text\">Fig. 3<\/b><img decoding=\"async\" aria-describedby=\"figure-3-desc\" src=\"https:\/\/www.europesays.com\/ie\/wp-content\/uploads\/2026\/11\/41598_2026_75938_Fig3_HTML.png\" alt=\"Fig. 3\" loading=\"lazy\" width=\"685\" height=\"515\"\/><\/p>\n<p>Effect of irradiation dose on the mechanical properties of LDPE\/PVB\/Bi2O3 nanocomposite: (<b>a<\/b>) tensile strength, (<b>b<\/b>) elongation at break, and (<b>c<\/b>) elastic modulus.<\/p>\n<p>Effect of EB-irradiation on gel fraction and crosslink density<\/p>\n<p>The effect of irradiation dose on the gel fraction of the LDPE\/PVB\/Bi2O3 nanocomposite is shown in Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig4\" rel=\"nofollow noopener\" target=\"_blank\">4<\/a>a. The gel fraction increases markedly with increasing irradiation dose from 10 to 100\u00a0kGy, followed by a nearly constant value at higher doses (120\u2013150\u00a0kGy). The unirradiated sample exhibits a very low gel fraction of about 5%. As the irradiation dose increases to 10, 30, 50, and 100\u00a0kGy, the gel fraction increases to approximately 17, 38, 67, and 92%, respectively. Above 100\u00a0kGy, only a slight increase is observed, reaching 93\u201394% at 125\u2013150\u00a0kGy. The initial increase in gel fraction is attributed to radiation-induced generation of macroradicals along the LDPE\/PVB polymer chains. These subsequently recombine to form intermolecular crosslinks and progressively develop a three-dimensional polymer network. The presence of the polar PVB may also contribute to the development of the network because irradiation can generate reactive sites in the polymer blend, facilitating intermolecular reactions between the constituent chains. Similar dose-dependent increases in gel fraction have been reported for irradiated polyethylene, where increasing irradiation dose promotes the formation of a crosslinked network<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 42\" title=\"Mitsui, H., Hosoi, F. &amp; Kagiya, T. &#x3B3;-radiation-induced cross-linking of polyethylene. Polym. J. 4, 79&#x2013;86 (1973).\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#ref-CR42\" id=\"ref-link-section-d3355104e1108\" rel=\"nofollow noopener\" target=\"_blank\">42<\/a>.<\/p>\n<p>The crosslink density of the LDPE\/PVB\/Bi2O3 nanocomposite increased with increasing EB irradiation dose, indicating progressive formation of a three-dimensional crosslinked network within the polymer matrix as shown in Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig4\" rel=\"nofollow noopener\" target=\"_blank\">4<\/a>b. The enhanced crosslink density restricts molecular-chain mobility and improves the structural integrity of the composite. At higher irradiation doses, the crosslink density tends to approach a plateau, suggesting that most available reactive sites have been consumed and further irradiation produces only a limited increase in network formation. Overall, the results confirm that irradiation effectively promotes crosslinking of the LDPE\/PVB\/Bi2O3 nanocomposite at 100\u00a0kGy, providing a highly developed crosslinked structure, which is considered an optimum dose for achieving a highly crosslinked LDPE\/PVB\/Bi2O3 nanocomposite. Studies on irradiated LDPE have shown that increasing radiation dose increases crosslink density.<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 43\" title=\"Gheysari, D. &amp; Behjat, A. Radiation crosslinking of LDPE and HDPE with 5 and 10&#xA0;MeV electron beams. Eur. Polymer J. 37, 2011&#x2013;2016 (2001).\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#ref-CR43\" id=\"ref-link-section-d3355104e1131\" rel=\"nofollow noopener\" target=\"_blank\">43<\/a> Additionally, the results are consistent with previous reports that EB irradiation increased crosslink density and improved interfacial interaction after irradiation.<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 44\" title=\"Ismail, N. H., Mustapha, M., Ismail, H., Jamil, M. K. &amp; Hairaldin, S. Z. Effect of electron beam irradiation on dielectric properties, morphology and melt rheology of linear low density polyethylene\/silicone rubber-based thermoplastic elastomer nanocomposites. Polym. Eng. Sci. 58, E135&#x2013;E144 (2018).\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#ref-CR44\" id=\"ref-link-section-d3355104e1135\" rel=\"nofollow noopener\" target=\"_blank\">44<\/a><\/p>\n<p>Figure <a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig5\" rel=\"nofollow noopener\" target=\"_blank\">5<\/a> presents the schematic mechanism of interaction among LDPE, PVB, and Bi2O3 nanoparticles under EB irradiation. Irradiation induces bond scission in both LDPE and PVB chains, generating reactive polymer radicals. These radicals follow three principal pathways: LDPE\u2013LDPE crosslinking via radical recombination, LDPE\u2013PVB coupling that enhances polymer\u2013polymer compatibility, and interfacial bonding between PVB hydroxyl groups and Bi2O3 nanoparticles through hydrogen bonding\/coordination. Collectively, these processes yield a dense, integrated polymeric network reinforced by Bi2O3 nanoparticles, which improves structural properties and enhances the physicochemical performance of the LDPE\/PVB\/Bi2O3 nanocomposite.<\/p>\n<p><b id=\"Fig4\" class=\"c-article-section__figure-caption\" data-test=\"figure-caption-text\">Fig. 4<\/b><img decoding=\"async\" aria-describedby=\"figure-4-desc\" src=\"https:\/\/www.europesays.com\/ie\/wp-content\/uploads\/2026\/11\/41598_2026_75938_Fig4_HTML.png\" alt=\"Fig. 4\" loading=\"lazy\" width=\"685\" height=\"246\"\/><\/p>\n<p>Effect of EB irradiation dose on the gel fraction (%) and crosslinking density of LDPE\/PVB\/Bi2O3 nanocomposites.<\/p>\n<p><b id=\"Fig5\" class=\"c-article-section__figure-caption\" data-test=\"figure-caption-text\">Fig. 5<\/b><img decoding=\"async\" aria-describedby=\"figure-5-desc\" src=\"https:\/\/www.europesays.com\/ie\/wp-content\/uploads\/2026\/11\/41598_2026_75938_Fig5_HTML.png\" alt=\"Fig. 5\" loading=\"lazy\" width=\"685\" height=\"370\"\/><\/p>\n<p>Schematic mechanism of interaction of LDPE, PVB, and Bi2O3 nanoparticles during EB irradiation.<\/p>\n<p>FTIR results<\/p>\n<p>Figure <a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig6\" rel=\"nofollow noopener\" target=\"_blank\">6<\/a> presents the FTIR spectra of LDPE, PVB, LDPE\/PVB (95\/5) blend, and irradiated LDPE\/PVB\/Bi2O3 nanocomposite. The FTIR spectrum of neat LDPE (Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig6\" rel=\"nofollow noopener\" target=\"_blank\">6<\/a>a) exhibits the characteristic absorption bands of polyethylene. The strong peaks observed at 2916 and 2848\u00a0cm\u2212\u20091 correspond to the asymmetric and symmetric stretching vibrations of \u2013CH\u2082 groups, respectively. The bands at around 1463\u00a0cm\u2212\u20091 and 720\u00a0cm\u2212\u20091 are attributed to CH\u2082 bending (scissoring) and rocking vibrations of long-chain methylene groups, confirming the typical molecular structure of LDPE<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 45\" title=\"Gulmine, J. V., Janissek, P. R., Heise, H. M. &amp; Akcelrud, L. Polyethylene characterization by FTIR. Polym. Test. 21, 557&#x2013;563 (2002).\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#ref-CR45\" id=\"ref-link-section-d3355104e1236\" rel=\"nofollow noopener\" target=\"_blank\">45<\/a>. The spectrum of PVB (Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig6\" rel=\"nofollow noopener\" target=\"_blank\">6<\/a>b) displays several characteristic absorption bands associated with its functional groups. A broad absorption band centered around 3440\u00a0cm\u2212\u20091 is assigned to the stretching vibration of hydroxyl (\u2013OH) groups. The peaks near 2930\u20132870\u00a0cm\u2212\u20091 correspond to aliphatic C\u2013H stretching vibrations. The absorption band observed around 1724\u00a0cm\u2212\u20091 is attributed to the carbonyl (C\u2009=\u2009O) stretching of residual vinyl acetate groups. The absorption band near 1450\u00a0cm\u2212\u20091 is assigned to C\u2013H bending vibrations of methylene and methyl groups, while bands in the range of 1100\u20131000\u00a0cm\u2212\u20091 are associated with C\u2013O\u2013C and C\u2013O stretching vibrations of the butyral structure. These characteristic absorption bands collectively confirm the presence of butyral acetal, hydroxyl, and acetate functionalities of PVB<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" title=\"Koysuren, O., Karaman, M. &amp; Dinc, H. Preparation and characterization of polyvinyl borate\/polyvinyl alcohol (PVB\/PVA) blend nanofibers. J. Appl. Polym. Sci. 124, 2736&#x2013;2741 (2012).\" href=\"#ref-CR46\" id=\"ref-link-section-d3355104e1254\">46<\/a>,<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" title=\"Wang, C. et al. Synthesis, solvent interactions and Hansen solubility parameters of polyvinyl butyral. Polym. Bull. 80, 6363&#x2013;6383 (2023).\" href=\"#ref-CR47\" id=\"ref-link-section-d3355104e1254_1\">47<\/a>,<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 48\" title=\"Nikitakos, V., Razos, C., Porfyris, A. D., Papaspyrides, C. D. &amp; Beltsios, K. G. Poly (vinyl butyral) Composites with Different Silicate or Silica Dispersions. Polymers 18, 476 (2026).\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#ref-CR48\" id=\"ref-link-section-d3355104e1257\" rel=\"nofollow noopener\" target=\"_blank\">48<\/a>. In the FTIR spectrum of the LDPE\/PVB (95\/5) blend (Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig6\" rel=\"nofollow noopener\" target=\"_blank\">6<\/a>c), the incorporation of PVB introduces several additional absorption bands associated with its functional groups. In addition, the spectrum contains the principal absorption bands of both LDPE and PVB, indicating successful blending between them. Slight broadening and minor shifts in some absorption bands suggest intermolecular interactions between the hydroxyl groups of PVB and the polyethylene matrix. The characteristic CH\u2082 stretching bands of LDPE appeared at 2916 and 2848\u00a0cm\u2212\u20091, while the broad hydroxyl band of PVB appeared with reduced intensity due to its lower concentration in the blend. The presence of both polymer-specific bands. In addition, the band observed near 1463\u00a0cm\u22121is assigned to CH\u2082 bending (scissoring) vibrations, while the characteristic CH\u2082 rocking vibration appearing around 723\u00a0cm\u2212\u20091 serves as a fingerprint band for polyethylene crystallinity. The characteristic PVB peaks appearing at 1132\u00a0cm\u2212\u20091 and 995\u00a0cm\u2212\u20091 correspond to the C\u2013O\u2013C stretching vibration of the butyral ring and C\u2013O stretching vibrations, respectively, confirming the presence of acetal functionalities in the blend. Furthermore, the absorption band observed near 1698\u00a0cm\u2212\u20091 is assigned to the C\u2009=\u2009O stretching vibration of residual vinyl acetate groups. Another band detected around 1377\u00a0cm\u2212\u20091 represents a characteristic polyolefin-related vibration associated with LDPE<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 19\" title=\"Jab&#x142;o&#x144;ska, B., Pozna&#x144;ska, G., Jab&#x142;o&#x144;ski, P. &amp; Zwoli&#x144;ska, J. Thermochemical valorization of plastic waste containing low density polyethylene, polyvinyl chloride and polyvinyl butyral into thermal and fuel energy. Energies 17, 3458 (2024).\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#ref-CR19\" id=\"ref-link-section-d3355104e1280\" rel=\"nofollow noopener\" target=\"_blank\">19<\/a>. The FTIR spectrum of the LDPE\/PVB\/ Bi2O3 nanocomposite (Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig6\" rel=\"nofollow noopener\" target=\"_blank\">6<\/a>d) retains the characteristic absorption bands of the LDPE\/PVB blend, indicating that the fundamental chemical structures of both polymers remain unchanged after incorporation of Bi2O3 nanoparticles. The FTIR spectrum of PVB exhibits characteristic absorption bands at 1132 and 995\u00a0cm\u207b\u00b9, corresponding to C\u2013O stretching vibrations. Upon incorporation of Bi2O3 nanoparticles, slight changes in band intensity and small shifts are observed in the hydroxyl and C\u2013O stretching regions. These spectral modifications reflect specific interactions between Bi2O3 and the functional groups of PVB, indicating successful integration of the nanoparticles within the polymer matrix. Furthermore, the appearance or enhancement of weak absorption bands in the 500\u2013650\u00a0cm\u2212\u20091 region can be attributed to Bi\u2013O stretching vibrations, confirming the successful incorporation of Bi2O3 nanoparticles within the polymer matrix<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 49\" title=\"Abdel Maksoud, M. I. A., Fahim, R. A., Kassem, S. M. &amp; Awed, A. S. Gamma irradiation-induced changes in structural, linear\/nonlinear optical, and optoelectrical properties of PVB\/BiVO4 nanocomposite for organic electronic devices. Opt. Quant. Electron. 55, 1165 (2023).\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#ref-CR49\" id=\"ref-link-section-d3355104e1311\" rel=\"nofollow noopener\" target=\"_blank\">49<\/a>. The absence of new major absorption bands indicates that the nanoparticles are physically dispersed within the blend rather than chemically altering the polymer backbone. Additionally, EB irradiation can improve interfacial interaction between components, enhance nanoparticle dispersion, and increase crosslink density, leading to improved mechanical, thermal, and surface properties.<\/p>\n<p><b id=\"Fig6\" class=\"c-article-section__figure-caption\" data-test=\"figure-caption-text\">Fig. 6<\/b><img decoding=\"async\" aria-describedby=\"figure-6-desc\" src=\"https:\/\/www.europesays.com\/ie\/wp-content\/uploads\/2026\/11\/41598_2026_75938_Fig6_HTML.png\" alt=\"Fig. 6\" loading=\"lazy\" width=\"685\" height=\"814\"\/><\/p>\n<p>FTIR spectrum of (<b>a<\/b>) LDPE, (<b>b<\/b>) PVB, (<b>c<\/b>) LDPE\/PVB blend (95\/5), and (<b>d<\/b>) LDPE\/PVB\/Bi2O3 nanocomposite.<\/p>\n<p>XRD results<\/p>\n<p>Figure <a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig7\" rel=\"nofollow noopener\" target=\"_blank\">7<\/a> represents the XRD patterns of LDPE, PVB, LDPE\/PVB blend, LDPE\/PVB\/Bi2O3, and irradiated LDPE\/PVB\/Bi2O3 nanocomposite at 100\u00a0kGy, which provide important information about the crystalline structure and phase distribution of the prepared materials. The patterns clearly demonstrate the coexistence of the crystalline LDPE phase, the predominantly amorphous PVB phase, and the crystalline Bi2O3 phase, together with structural modifications induced by electron-beam irradiation.<\/p>\n<p>Neat LDPE (Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig7\" rel=\"nofollow noopener\" target=\"_blank\">7<\/a>a) exhibits two intense and well-defined diffraction peaks at 2\u03b8\u2009=\u200921.4\u00b0 and 23.7\u00b0, which are assigned to the (110) and (200) planes, respectively, of the crystalline structure of LDPE. The pronounced intensity of these reflections confirms the semicrystalline nature of LDPE<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" title=\"Roy, P. K., Surekha, P., Rajagopal, C., Chatterjee, S. N. &amp; Choudhary, V. Studies on the photo-oxidative degradation of LDPE films in the presence of oxidised polyethylene. Polym. Degrad. Stab. 92, 1151&#x2013;1160 (2007).\" href=\"#ref-CR50\" id=\"ref-link-section-d3355104e1382\">50<\/a>,<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" title=\"Hamouya, M., Mahir, A. &amp; Idrissi, M. C. E. L. Natural ageing of stabilized and unstabilized Ldpe Films: Xrd and Sem Analysis. relation 7, 9 (2014).\" href=\"#ref-CR51\" id=\"ref-link-section-d3355104e1382_1\">51<\/a>,<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 52\" title=\"Depan, D., Chirdon, W. &amp; Khattab, A. Morphological and chemical analysis of low-density polyethylene crystallized on carbon and clay nanofillers. Polymers 13, 1558 (2021).\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#ref-CR52\" id=\"ref-link-section-d3355104e1385\" rel=\"nofollow noopener\" target=\"_blank\">52<\/a>. In contrast, the XRD pattern of PVB (Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig7\" rel=\"nofollow noopener\" target=\"_blank\">7<\/a>b) shows a broad diffraction halo centered around 2\u03b8\u2009\u2248\u200919.2\u00b0. This broad feature is characteristic of the predominantly amorphous structure of PVB<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 53\" title=\"Kumar, P., Khan, N. &amp; Kumar, D. Polyvinyl butyral (PVB), versetile template for designing nanocomposite\/composite materials: A review. Green. Chem. Technol. Lett. 2, 185&#x2013;194 (2016).\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#ref-CR53\" id=\"ref-link-section-d3355104e1392\" rel=\"nofollow noopener\" target=\"_blank\">53<\/a>,<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 54\" title=\"Zhang, Y., Ding, Y., Li, Y., Gao, J. &amp; Yang, J. Synthesis and characterization of polyvinyl butyral&#x2013;Al (NO3) 3 composite sol used for alumina based fibers. J. Solgel Sci. Technol. 49, 385&#x2013;390 (2009).\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#ref-CR54\" id=\"ref-link-section-d3355104e1395\" rel=\"nofollow noopener\" target=\"_blank\">54<\/a>. Upon blending PVB with LDPE, the LDPE characteristic (110) and (200) reflections remain visible in the XRD pattern of the LDPE\/PVB blend (Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig7\" rel=\"nofollow noopener\" target=\"_blank\">7<\/a>c), indicating that incorporation of PVB does not destroy the basic crystalline structure of LDPE. However, the relative intensity and broadness of the diffraction profile are modified because of the contribution of the amorphous PVB phase and interactions between the two polymer components. This suggests that the LDPE crystalline domains are retained within the polymer blend with good compatibility between LDPE and PVB.<\/p>\n<p>Upon incorporation of Bi2O3, the LDPE\/PVB\/Bi2O3 nanocomposite (Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig7\" rel=\"nofollow noopener\" target=\"_blank\">7<\/a>d) retained the characteristic crystalline peaks of LDPE, while exhibiting slight peak broadening and reduced diffraction intensity. In addition, weak diffraction features corresponding to Bi2O3 nanoparticles appeared, confirming their successful incorporation into the polymer matrix. These changes can be attributed to the homogeneous nanoscale dispersion of Bi2O3 nanoparticles and are consistent with enhanced interfacial compatibility with the LDPE\/PVB polymer chains, which slightly modified the crystalline arrangement of the composite system.<\/p>\n<p>For the LDPE\/PVB\/Bi2O3 nanocomposite (Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig7\" rel=\"nofollow noopener\" target=\"_blank\">7<\/a>d), the characteristic LDPE reflections remain evident, while additional weaker reflections appear at higher diffraction angles and are assigned to the crystalline Bi\u2082O\u2083 phase, including the indexed reflections shown in the figure, such as (002), (200), (211), and (122). The simultaneous presence of the LDPE and Bi\u2082O\u2083 reflections confirms the successful incorporation of the inorganic oxide into the polymer matrix. The absence of a substantial amorphous background increase or disappearance of the principal LDPE peaks indicates that Bi2O3 incorporation does not completely disrupt the semicrystalline structure of LDPE. After EB irradiation of the LDPE\/PVB\/Bi2O3 nanocomposite at 100\u00a0kGy (Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig6\" rel=\"nofollow noopener\" target=\"_blank\">6<\/a>e), the main LDPE reflections are still observed, demonstrating that the fundamental crystalline structure of the LDPE matrix is preserved after irradiation. At the same time, several additional Bi\u2082O\u2083-related reflections become more distinguishable, including the indexed (002), (200), (220), <b>(<\/b>121), (122), (222), (141), and (004) reflections. The persistence of these characteristic oxide reflections confirms the structural stability of the Bi2O3 nanoparticles during electron-beam processing. Therefore, the XRD results support the formation of an LDPE\/PVB\/Bi\u2082O\u2083 nanocomposite in which the LDPE crystalline phase and Bi\u2082O\u2083 crystalline phase are maintained, while electron-beam irradiation primarily modifies the polymer network through radiation-induced crosslinking rather than producing a new crystalline phase, supporting the formation of a stable crosslinked LDPE\/PVB\/Bi2O3 nanocomposite.<\/p>\n<p><b id=\"Fig7\" class=\"c-article-section__figure-caption\" data-test=\"figure-caption-text\">Fig. 7<\/b><img decoding=\"async\" aria-describedby=\"figure-7-desc\" src=\"https:\/\/www.europesays.com\/ie\/wp-content\/uploads\/2026\/11\/41598_2026_75938_Fig7_HTML.png\" alt=\"Fig. 7\" loading=\"lazy\" width=\"685\" height=\"876\"\/><\/p>\n<p>XRD curves of (<b>a<\/b>) LDPE, (<b>b<\/b>) PVB, (<b>c<\/b>) LDPE\/PVB blend, (<b>d<\/b>) unirradiated LDPE\/PVB\/Bi2O3, (<b>e<\/b>) LDPE\/PVB\/Bi2O3 nanocomposite irradiated at 100\u00a0kGy.<\/p>\n<p>Surface morphology<\/p>\n<p>The SEM micrographs in Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig8\" rel=\"nofollow noopener\" target=\"_blank\">8<\/a> show the morphological evolution of LDPE after incorporation of PVB, Bi2O3 nanoparticles, and subsequent electron-beam irradiation at 100\u00a0kGy. The SEM micrograph of neat LDPE (Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig8\" rel=\"nofollow noopener\" target=\"_blank\">8<\/a>a) reveals a relatively smooth, compact, and homogeneous surface. The absence of pronounced cracks, voids, or phase-separated domains highlights the uniform morphology, good structural integrity, and stable polymeric nature of the LDPE matrix. This smooth appearance further reflects its ductile character and excellent film-forming capability.<\/p>\n<p>Figure <a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig8\" rel=\"nofollow noopener\" target=\"_blank\">8<\/a>b shows the SEM of LDPE\/PVB after incorporation of 5 wt% PVB into LDPE; the surface becomes rougher and more fibrillar in morphology, with elongated streaks and irregular surface features. Nevertheless, no large cavities or severe phase separation are apparent, indicating reasonably good compatibility between LDPE and PVB.<\/p>\n<p>Upon incorporation of Bi2O3 nanoparticles into the LDPE\/PVB blend (Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig8\" rel=\"nofollow noopener\" target=\"_blank\">8<\/a>c), the nanocomposite surface exhibits a more regulated morphology with uniformly distributed, highly dispersed nanoparticles. The absence of extensive agglomeration indicates effective nanoparticle dispersion within the polymer matrix, contributing to improved structural uniformity. Similar morphological characterization of LDPE\/Bi2O3 nanocomposites by SEM has demonstrated the influence of Bi2O3 incorporation on the surface morphology and filler dispersion within the polyethylene matrix.<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 55\" title=\"Alshahri, S. et al. LDPE\/bismuth oxide nanocomposite: Preparation, characterization and application in X-ray shielding. Polymers 13, 3081 (2021).\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#ref-CR55\" id=\"ref-link-section-d3355104e1547\" rel=\"nofollow noopener\" target=\"_blank\">55<\/a>.<\/p>\n<p>After irradiation, the SEM of LDPE\/PVB\/Bi2O3 at 100\u00a0kGy (Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig8\" rel=\"nofollow noopener\" target=\"_blank\">8<\/a>d) shows that the nanocomposite exhibits a more compact and relatively homogeneous morphology, with a reduction in pronounced grooves and surface defects compared with the non-irradiated nanocomposite. The smoother morphology can be attributed to EB-induced crosslinking, which promotes intermolecular bonding and network formation within the polymer matrix. The resulting crosslinked structure can restrict polymer-chain mobility, improve interfacial interactions among LDPE, PVB, and Bi2O3, and reduce the development of voids or interfacial defects. The improved morphological integrity is therefore consistent with the enhanced mechanical and radiation-resistant properties of the irradiated nanocomposite. The results are consistent with LDPE\/Bi2O3 nanocomposites, as confirmed by SEM analysis, which effectively demonstrates Bi2O3 nanoparticle dispersion and the resulting surface morphology.<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 55\" title=\"Alshahri, S. et al. LDPE\/bismuth oxide nanocomposite: Preparation, characterization and application in X-ray shielding. Polymers 13, 3081 (2021).\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#ref-CR55\" id=\"ref-link-section-d3355104e1574\" rel=\"nofollow noopener\" target=\"_blank\">55<\/a>.<\/p>\n<p><b id=\"Fig8\" class=\"c-article-section__figure-caption\" data-test=\"figure-caption-text\">Fig. 8<\/b><img decoding=\"async\" aria-describedby=\"figure-8-desc\" src=\"https:\/\/www.europesays.com\/ie\/wp-content\/uploads\/2026\/11\/41598_2026_75938_Fig8_HTML.png\" alt=\"Fig. 8\" loading=\"lazy\" width=\"685\" height=\"521\"\/><\/p>\n<p>SEM micrographs of (<b>a<\/b>) neat LDPE, (<b>b<\/b>) LDPE\/PVB (95\/5) blend, (<b>c<\/b>) LDPE\/PVB\/Bi2O3 nanocomposite, and (<b>d<\/b>) irradiated LDPE\/PVB\/Bi2O3 nanoconposite at 100\u00a0kGy.<\/p>\n<p>Thermal stability<\/p>\n<p>Figure <a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig9\" rel=\"nofollow noopener\" target=\"_blank\">9<\/a> represents the TGA curves of LDPE, LDPE\/PVB, LDPE\/PVB\/Bi2O3, and irradiated LDPE\/PVB\/Bi2O3 nanocomposite at 100\u00a0kGy, demonstrating the influence of PVB blending, Bi2O3 nanoparticles, and EB irradiation on the thermal stability of LDPE-based composites. The TGA curves reveal the thermal degradation behavior of four material systems over a temperature range of 30\u00a0\u00b0C to 600\u00a0\u00b0C. All samples remain thermally stable up to around 200\u2013250\u00a0\u00b0C, showing negligible mass loss during this initial stage. The neat LDPE sample exhibits the lowest thermal stability, showing an earlier onset of degradation and rapid weight loss within the temperature range of 330\u2013470\u00a0\u00b0C due to the thermal decomposition of polyethylene chains, leaving a residual mass of 2\u20133%. After blending with PVB, the LDPE\/PVB composite displays improved thermal resistance, as evidenced by the shift of the degradation curve toward higher temperatures and the slower decomposition rate. This enhancement suggests that the incorporation of PVB provides a modest improvement in thermal stability compared with pure LDPE, attributed to the improved intermolecular interactions within the LDPE\/PVB polymer matrix.<\/p>\n<p>The incorporation of Bi2O3 nanoparticles into the LDPE\/PVB matrix further enhances the thermal stability of the composite. The LDPE\/PVB\/Bi2O3 sample shows a delayed degradation process and weight loss within the temperature range of 430\u00a0\u00b0C and higher, with residual mass at elevated temperatures, indicating that Bi2O3 nanoparticles act as thermal barriers that restrict the mobility of polymer chains and retard the diffusion of volatile decomposition products. Moreover, the nanoparticles may promote char formation and improve heat dissipation during thermal decomposition. The irradiated LDPE\/PVB\/Bi2O3 nanocomposite at 100\u00a0kGy exhibits the highest thermal stability among all investigated samples. The TGA curve shifts noticeably toward higher temperatures, with a slower and more gradual weight loss process. This behavior suggests that irradiation at 100\u00a0kGy induces crosslinking within the polymer matrix, enhancing intermolecular bonding and reducing chain scission. In addition, the synergistic effect of irradiation and Bi2O3 nanoparticles contributes to the formation of a more compact and thermally resistant network structure. Consequently, the irradiated nanocomposite retains a higher percentage of its mass at elevated temperatures, confirming its superior thermal durability and resistance to thermal degradation.<\/p>\n<p><b id=\"Fig9\" class=\"c-article-section__figure-caption\" data-test=\"figure-caption-text\">Fig. 9<\/b><img decoding=\"async\" aria-describedby=\"figure-9-desc\" src=\"https:\/\/www.europesays.com\/ie\/wp-content\/uploads\/2026\/11\/41598_2026_75938_Fig9_HTML.png\" alt=\"Fig. 9\" loading=\"lazy\" width=\"685\" height=\"502\"\/><\/p>\n<p>TGA curves of neat LDPE, LDPE\/PVB blend, LDPE\/PVB\/Bi2O3 unirradiated, and irradiated LDPE\/PVB\/Bi2O3 nanocomposite irradiated at 100\u00a0kGy.<\/p>\n<p>Contact angle measurement<\/p>\n<p>The surface hydrophobicity of materials can be quantitatively evaluated by measuring the water contact angle, which provides a direct indication of surface wettability. A lower contact angle corresponds to greater water spreading and, consequently, higher surface wettability and lower hydrophobicity, whereas a higher contact angle indicates reduced wettability, enhanced hydrophobicity, and greater water repellency. A contact angle less than 90\u00b0 indicates a hydrophilic surface, meaning the surface has a high affinity for water and allows the droplet to spread more readily. In contrast, a contact angle greater than 90\u00b0 indicates a hydrophobic surface, reflecting a lower affinity for water and a more spherical droplet shape. Therefore, an increase in contact angle corresponds to an increase in the hydrophobicity of the surface, while a decrease in contact angle indicates greater surface wettability.<\/p>\n<p>The contact angle measurements presented in Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig10\" rel=\"nofollow noopener\" target=\"_blank\">10<\/a> clearly demonstrate the effects of PVB incorporation, Bi2O3 nanoparticle addition, and EB irradiation on the surface wettability and hydrophobicity of the LDPE-based composites. The neat LDPE film exhibits a contact angle of 93\u00b0<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 56\" title=\"Aktas, C. et al. Force-based characterization of the wetting properties of LDPE surfaces treated with CF4 and H2 plasmas. Polymers 15, 2132 (2023).\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#ref-CR56\" id=\"ref-link-section-d3355104e1714\" rel=\"nofollow noopener\" target=\"_blank\">56<\/a>, indicating its intrinsically hydrophobic nature, which can be attributed to its nonpolar hydrocarbon backbone and relatively low surface energy. As observed in the inset photograph, the water droplet retains a relatively hemispherical shape with limited spreading across the LDPE surface, confirming its moderate water repellency and low surface wettability.<\/p>\n<p>Following blending of LDPE with PVB, the contact angle of LDPE\/PVB increases to 112\u00b0, indicating a clear enhancement in surface hydrophobicity compared with the pristine LDPE film. This increase may be attributed to the alteration of surface morphology and intermolecular interactions arising from the incorporation of PVB, which can modify the surface roughness and chemical characteristics of the blend.<\/p>\n<p>The incorporation of Bi2O3 nanoparticles into the LDPE\/PVB matrix at 0\u00a0kGy increases the water contact angle to 124\u00b0, indicating a pronounced enhancement in surface hydrophobicity. This improvement can be attributed to the presence of Bi2O3 nanoparticles enhance the surface stability of the composite and contribute to reduced surface wettability. This result is consistent with previous studies reporting that the incorporation of nanoparticles into polymeric composite films can increase surface roughness and hydrophobicity, thereby leading to an increase in the water contact angle.<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 57\" title=\"Khorasani, M. T., Joorabloo, A., Moghaddam, A., Shamsi, H. &amp; MansooriMoghadam, Z. Incorporation of ZnO nanoparticles into heparinised polyvinyl alcohol\/chitosan hydrogels for wound dressing application. Int. J. Biol. Macromol. 114, 1203&#x2013;1215 (2018).\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#ref-CR57\" id=\"ref-link-section-d3355104e1732\" rel=\"nofollow noopener\" target=\"_blank\">57<\/a><\/p>\n<p>After EB irradiation at 100\u00a0kGy, the LDPE\/PVB\/Bi2O3 nanocomposite exhibits the highest water contact angle of 142\u00b0, indicating a pronounced enhancement in surface hydrophobicity and water-repellent behavior, which consequently suggests improved self-cleaning potential. This behavior can be attributed to the synergistic effect between Bi2O3 nanoparticles and EB irradiation, while promote the formation of hierarchical surface features, further reducing water-surface interactions and enhancing water repellency. Overall, the contact angle results confirm that the incorporation of PVB and Bi2O3 nanoparticles, combined with EB irradiation, significantly improves the hydrophobicity and potential self-cleaning properties of the LDPE-based nanocomposites.<\/p>\n<p>The inset photographs show a small water droplet deposited on the surfaces of the LDPE-based samples to evaluate their surface wettability, with the contact angle determined at the three-phase contact line between the droplet and the solid surface. The droplets exhibit increasingly rounded, dome-like shapes with increasing contact angle, indicating progressively reduced water spreading and enhanced hydrophobicity. The contact angle increased from 95\u00b0 for LDPE to 108\u00b0 for LDPE\/PVB and 121\u00b0 for the unirradiated LDPE\/PVB\/Bi2O3 nanocomposite, while irradiation at 100\u00a0kGy further increased the contact angle to 139\u00b0, producing the most pronounced droplet curvature and the lowest surface wettability. These photographic observations are in good agreement with the measured contact-angle values, confirming the progressive enhancement of the water-repellent character of the nanocomposite surface.<\/p>\n<p><b id=\"Fig10\" class=\"c-article-section__figure-caption\" data-test=\"figure-caption-text\">Fig. 10<\/b><img decoding=\"async\" aria-describedby=\"figure-10-desc\" src=\"https:\/\/www.europesays.com\/ie\/wp-content\/uploads\/2026\/11\/41598_2026_75938_Fig10_HTML.png\" alt=\"Fig. 10\" loading=\"lazy\" width=\"685\" height=\"492\"\/><\/p>\n<p>Contact angle measurements of LDPE film, LDPE\/PVB, the unirradiated LDPE\/PVB\/Bi2O3, and the irradiated LDPE\/PVB\/Bi2O3 at 100\u00a0kGy.<\/p>\n<p>Self-cleaning performance<\/p>\n<p>Figure <a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig11\" rel=\"nofollow noopener\" target=\"_blank\">11<\/a> depicts the self-cleaning performance of LDPE, LDPE\/PVB, LDPE\/PVB\/Bi2O3, and irradiated LDPE\/PVB\/Bi2O3 nanocomposite, evaluated through the photodegradation of MB dye under UV irradiation. As shown in Fig.\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig11\" rel=\"nofollow noopener\" target=\"_blank\">11<\/a>A, the degradation efficiency of pristine LDPE reaches only 16% after 8\u00a0h of UV irradiation, whereas LDPE\/PVB achieves 48%. Incorporation of Bi2O3 nanoparticles markedly enhances the efficiency to 83%, underscoring their effective photocatalytic role in generating reactive oxygen species that decompose organic dye molecules. Notably, the irradiated LDPE\/PVB\/Bi2O3 nanocomposite exhibits the highest performance, approaching 94% degradation after 8\u00a0h of irradiation. The enhanced photocatalytic self-cleaning performance of the irradiated nanocomposite arises from multiple synergistic factors. First, Bi2O3 nanoparticles serve as active photocatalytic centers, absorbing UV light and generating electron\u2013hole pairs that subsequently yield highly reactive radicals responsible for dye degradation. Second, irradiation treatment improves nanoparticle dispersion and strengthens interfacial interaction within the polymer matrix, thereby increasing the density of accessible active sites, facilitating charge separation, and suppressing electron\u2013hole recombination. Consequently, the irradiated LDPE\/PVB\/Bi2O3 nanocomposite exhibits markedly superior photocatalytic efficiency and self-cleaning capability. Figure\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"figure anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Fig11\" rel=\"nofollow noopener\" target=\"_blank\">11<\/a>B presents photographic images showing the progressive discoloration of MB dye on the sample surfaces as a function of UV irradiation time. Upon UV exposure, the intensity of the blue coloration gradually decreases; however, the rate of dye removal strongly depends on the composition of the tested material. Pristine LDPE exhibits the lowest self-cleaning activity, retaining a considerable fraction of the dye even after 8\u00a0h of irradiation. Incorporation of PVB slightly improves stain degradation, producing a more noticeable reduction in color intensity compared with neat LDPE. A substantial enhancement is achieved with the addition of Bi2O3 nanoparticles, where the stain fades rapidly and becomes nearly invisible after extended irradiation. The irradiated LDPE\/PVB\/ Bi2O3 nanocomposite demonstrates the most pronounced self-cleaning behavior, with near-complete disappearance of the MB stain after only 4\u00a0h of UV exposure, confirming its superior photocatalytic activity. This improvement was attributed to the enhanced generation of reactive species, improved nanoparticle dispersion, and irradiation-induced surface modifications.<\/p>\n<p>The photocatalytic efficiency obtained for the irradiated LDPE\/PVB\/Bi2O3 nanocomposite (94% MB degradation after 8\u00a0h of UV irradiation) is superior to many reported polymer-supported photocatalysts. For example, cellulose acetate membranes containing ZnO nanoparticles<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 58\" title=\"Abu-Dalo, M. A., Al-Rosan, S. A. &amp; Albiss, B. A. Photocatalytic degradation of methylene blue using polymeric membranes based on cellulose acetate impregnated with ZnO nanostructures. Polymers 13, 3451 (2021).\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#ref-CR58\" id=\"ref-link-section-d3355104e1846\" rel=\"nofollow noopener\" target=\"_blank\">58<\/a> degraded only about 30% of MB under UV irradiation and approximately 75% under simulated sunlight, indicating lower photocatalytic activity than that achieved in the present work. In addition, Bi2O3-containing photocatalysts have demonstrated excellent dye degradation capability, with Bi2O3\u2013Al2O3 nanocomposites<a data-track=\"click\" data-track-action=\"reference anchor\" data-track-label=\"link\" data-test=\"citation-ref\" aria-label=\"Reference 59\" title=\"Hakimi, M., Morvaridi, M., Hosseini, H. A. &amp; Alimard, P. Preparation, characterization, and photocatalytic activity of Bi2O3&#x2013;Al2O3 nanocomposite. Polyhedron 170, 523&#x2013;529 (2019).\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#ref-CR59\" id=\"ref-link-section-d3355104e1863\" rel=\"nofollow noopener\" target=\"_blank\">59<\/a> achieving nearly 90% MB degradation under optimized UV irradiation conditions. These comparisons suggest that the synergistic combination of Bi2O3 nanoparticles and EB irradiation in the present study provides a highly efficient strategy for developing multifunctional self-cleaning polymeric materials.<\/p>\n<p>Table (1) presents a comparison of different polymer-supported photocatalytic systems for MB degradation, revealing that performance is strongly influenced by both material composition and processing method. Cellulose acetate\/ZnO membranes exhibited only modest activity (~\u200930% MB removal under UV), underscoring the limited efficiency of simple ZnO incorporation. In contrast, Bi2O3\u2013Al2O3 nanocomposites achieved\u2009~\u200990% degradation under optimized UV conditions, highlighting the superior photocatalytic potential of bismuth oxide systems. PVC films embedded with Bi-based heterostructures have also been reported to provide self-cleaning and antibacterial properties, confirming the versatility of Bi-based photocatalysts in polymer matrices. Beyond these polymer supports, Bi-based powders and thin films (e.g., BiVO4, Bi2WO6, BiOX) have demonstrated high visible-light activity, while biorenewable nanocomposites offer sustainable adsorption\u2013photocatalysis synergy for immaculate water production. Building on these findings, the present work introduces LDPE\/PVB\/Bi2O3 nanocomposites fabricated by EB irradiation, which not only improved mechanical, thermal, and wettability properties but also achieved 94% MB degradation after 8\u00a0h UV exposure. This demonstrates that radiation processing can significantly enhance photocatalytic efficiency while simultaneously tailoring multifunctional properties, positioning the developed system as a promising candidate for advanced wastewater treatment applications (Table <a data-track=\"click\" data-track-label=\"link\" data-track-action=\"table anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Tab1\" rel=\"nofollow noopener\" target=\"_blank\">1<\/a>).<\/p>\n<p><b id=\"Fig11\" class=\"c-article-section__figure-caption\" data-test=\"figure-caption-text\">Fig. 11<\/b><img decoding=\"async\" aria-describedby=\"figure-11-desc\" src=\"https:\/\/www.europesays.com\/ie\/wp-content\/uploads\/2026\/11\/41598_2026_75938_Fig11_HTML.png\" alt=\"Fig. 11\" loading=\"lazy\" width=\"685\" height=\"785\"\/><\/p>\n<p>Self-cleaning performance of (a) LDPE, (b) LDPE\/PVB, (c) unirradiated LDPE\/PVB\/Bi2O3, and (d) irradiated LDPE\/PVB\/Bi2O3 at 100\u00a0kGy, evaluated by the photocatalytic degradation of MB dye under UV irradiation. (<b>A<\/b>) Degradation efficiency (%) as a function of irradiation time, and (<b>B<\/b>) photographic images illustrating the progressive discoloration of MB stains on the sample surfaces during UV exposure.<\/p>\n<p><b id=\"Tab1\" data-test=\"table-caption\">Table 1 Comparison of photocatalytic systems for MB degradation.<\/b>Photocatalytic kinetics<\/p>\n<p>The kinetics of photocatalytic degradation of MB were analysed using pseudo-first-order and pseudo-second-order models as expressed in Eqs.\u00a04\u20135.<\/p>\n<p>$$\\:\\text{ln}\\left({C}_{0}-{C}_{t}\\right)=\\:{K}_{1}t$$<\/p>\n<p>\n                    (4)\n                <\/p>\n<p>$$\\:\\frac{t}{{C}_{t}}=\\:\\frac{1}{{k}_{2}{{C}_{0}}^{2}}+\\:\\frac{t}{{C}_{0}}$$<\/p>\n<p>\n                    (5)\n                <\/p>\n<p>where C0 is the initial MB concentration, Ct is the MB concentration at time t, and k1 is the pseudo-first-order rate constant, and k2 is the pseudo-second-order rate constant.<\/p>\n<p>Table\u00a0<a data-track=\"click\" data-track-label=\"link\" data-track-action=\"table anchor\" href=\"http:\/\/www.nature.com\/articles\/s41598-026-75938-7#Tab2\" rel=\"nofollow noopener\" target=\"_blank\">2<\/a> shows that the pseudo-first-order kinetic model provides excellent linear fits, with correlation coefficients (R2) ranging from 0.985 to 0.998, indicating that the degradation of MB is predominantly governed by photocatalytic reaction kinetics. The apparent rate constant (k1) increased systematically from 0.073\u00a0h\u207b\u00b9 for neat LDPE to 0.351\u00a0h\u207b\u00b9 for the LDPE\/PVB\/Bi2O3 nanocomposite irradiated at 100\u00a0kGy, demonstrating that the incorporation of Bi\u2082O\u2083 and EB irradiation significantly enhances the MB degradation rate.<\/p>\n<p>The pseudo-second-order model also showed good agreement with the experimental data, with R2 values ranging from 0.981 to 0.996, indicating that adsorption and surface interactions also contribute to the overall MB degradation process. The increase in the corresponding k2 values with Bi\u2082O\u2083 incorporation and irradiation dose suggests enhanced interactions between MB molecules and the nanocomposite. Nevertheless, the slightly higher R2 values obtained for the pseudo-first-order model indicate that photocatalytic degradation is the predominant kinetic pathway, while adsorption likely plays a complementary role. Overall, the kinetic results demonstrate that EB irradiation effectively enhances the photocatalytic performance of LDPE\/PVB\/Bi2O3 nanocomposites at 100\u00a0kGy,<\/p>\n<p><b id=\"Tab2\" data-test=\"table-caption\">Table 2 Kinetic parameters using pseudo-first-order and pseudo-second-order models.<\/b><\/p>\n","protected":false},"excerpt":{"rendered":"Characterization of Bi2O3 nanoparticles Figure 1a presents the TEM micrograph of Bi2O3 nanoparticles, revealing the formation of a&hellip;\n","protected":false},"author":2,"featured_media":796519,"comment_status":"","ping_status":"","sticky":false,"template":"","format":"standard","meta":{"footnotes":"","_share_on_mastodon":"0"},"categories":[77],"tags":[331530,8284,18,331531,9656,1099,331532,19,17,331528,909,1100,22745,331534,331529,133,331533],"class_list":["post-796518","post","type-post","status-publish","format-standard","has-post-thumbnail","category-science","tag-bi2o3-nanoparticles","tag-chemistry","tag-eire","tag-electron-beam-irradiation","tag-engineering","tag-humanities-and-social-sciences","tag-hydrophobicity","tag-ie","tag-ireland","tag-ldpe","tag-materials-science","tag-multidisciplinary","tag-nanoscience-and-technology","tag-photocatalytic-activity","tag-pvb","tag-science","tag-self-cleaning-nanocomposites"],"share_on_mastodon":{"url":"https:\/\/pubeurope.com\/@ie\/117672322770697152","error":""},"_links":{"self":[{"href":"https:\/\/www.europesays.com\/ie\/wp-json\/wp\/v2\/posts\/796518","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/www.europesays.com\/ie\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/www.europesays.com\/ie\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/www.europesays.com\/ie\/wp-json\/wp\/v2\/users\/2"}],"replies":[{"embeddable":true,"href":"https:\/\/www.europesays.com\/ie\/wp-json\/wp\/v2\/comments?post=796518"}],"version-history":[{"count":0,"href":"https:\/\/www.europesays.com\/ie\/wp-json\/wp\/v2\/posts\/796518\/revisions"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/www.europesays.com\/ie\/wp-json\/wp\/v2\/media\/796519"}],"wp:attachment":[{"href":"https:\/\/www.europesays.com\/ie\/wp-json\/wp\/v2\/media?parent=796518"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/www.europesays.com\/ie\/wp-json\/wp\/v2\/categories?post=796518"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/www.europesays.com\/ie\/wp-json\/wp\/v2\/tags?post=796518"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}