Object of research

The main goal of the study was to investigate the influence of the type of binder on paint stability. In this research, 12 commercial and modified paints from 6 different producers containing 2 types of pigments were used: ultramarine blue and cadmium yellow. The Samples used in the investigation are listed in Table 1.

Table 1 Paint producers with binder contentChemical changes by ATR FTIR

FTIR spectra allowed us to observe chemical changes in the paint binder during the ageing process. FTIR spectra showing evaporation and oxidizing effects in paint binders. In Figs. 2–4, 7, 10 and 13 the infrared spectra of the ultramarine blue and cadmium yellow are presented. Differential spectra of ultramarine blue and cadmium yellow are shown in Figs. 5, 6, 8, 9, 11–13 and 15. The band appearing at 2800–3000 cm−1 is assigned to aliphatic C-H vibrations36. The band at 1700–1730 cm−1 originated from C=O ketone carbonyl groups, as a paint oxidation products9,41. The band observed at approximately 1420 and 1600 cm−1 in Arabic gum is attributed to symmetric and asymmetric COO− vibrations. However, the band at approximately 1600 cm−1 exhibits an overlap with a band originating from amide groups, which is also present within the same spectral range42. The sources of the strong band in the ultramarine IR spectra in the 980–1030 cm−1 range are Si-OH or Si-O-Si groups43,44. The main type of mineral encountered in ultramarine paints is sodalite45,46.

In Fig. 3, FTIR spectra of ultramarine blue Leningrad normalized to a band with a maximum at 984 cm−1 originating from Si-OH groups and cadmium yellow Leningrad normalized to a band with a maximum at 2912 cm−1 assigned to C-H aliphatic groups were collected. The differential spectra are provided in the supplementary information file to facilitate a more detailed examination of the alterations depicted in Figs. S1 and S2. FTIR spectra of ultramarine blue were normalized to a band with a maximum at 984 cm−1 originating from Si-O groups and normalized to a band with a maximum at 2912 cm−1 assigned to C-H groups were collected. The analysis of the ultramarine blue samples subjected to thermal and light degradation revealed that it was not possible to register all the spectra due to the degradation and detachment of the paint from the glass. Therefore, there is no possibility to formulate a conclusion about chemical changes in the ultramarine Leningrad during thermal and light degradation. After 4 years of conditioning, an increase in the intensity of the band with a maximum at 1604 cm−1 originating from COO- groups was observed which indicated that the oxidation of Arabic gum with honey occurred. Figure S2 shows the differential FTIR spectra of cadmium yellow normalized to a band with a maximum at 2912 cm−1 originating from C-H aliphatic groups. The intensity of the band assigned to C-H groups decreased and the intensity of the band assigned to COO- groups increased, which confirmed the occurrence of Arabic gum evaporation and remnant oxidation. The results of the light degradation process indicate an increase in the intensity of the band due to COO- groups, which suggests that the Arabic gum underwent oxidation. These findings indicate that no observable degradation occurred during the 4-year ageing period. In general, the ultramarine blue Leningrad paint is less stable than the cadmium yellow.

Fig. 3: ATR FTIR spectra of ultramarine Leningrad normalized to a band originating from Si-OH groups with a maximum at 984 cm−1.Fig. 3: ATR FTIR spectra of ultramarine Leningrad normalized to a band originating from Si-OH groups with a maximum at 984 cm−1.The alternative text for this image may have been generated using AI.

a Thermally aged, T = 120 °C, b light aged, c conditioned for 4 years, and cadmium yellow Leningrad normalized to a band with a maximum at 2912 cm−1 assigned to C-H groups: d thermally aged, T = 120 °C, e light aged, f conditioned for 4 years.

Figure 4 presents FTIR spectra of ultramarine blue Schmincke normalized to the band with a maximum at 988 cm−1 originating from Si-OH groups (Fig. 4a–c) and cadmium yellow Schmincke normalized to the band with a maximum at 2917 cm−1 assigned to C-H groups (Fig. 4d–f). To facilitate a more comprehensive understanding of the alterations in question, the differential spectra depicted in Figs. S3 and S4, which are accessible via the supplementary information file, have been provided. During the thermal degradation of ultramarine blue (Fig. S3) a decrease in the intensity of the band due to C-H groups and an increase in the intensity of the band with a maximum at 1630 cm−1 assigned to COO- groups are observed. The results indicate that the Arabic gum with beef bile underwent both evaporation and oxidation. It is not possible to register the spectrum of ultramarine blue after 96 days of thermal degradation because the paint gives no FTIR signal. Despite this, the Schmincke ultramarine is demonstrably more stable than the Leningrad. A similar trend in the degradation process as that in the thermally aged sample can be observed for the ultramarine blue light aged paint, but the changes in the intensity of the bands indicating chemical changes are less significant. Ultramarine blue conditioning for 4 years did not significantly change the intensity of the bands due to the C-H and COO- groups. In Fig. S4 differential spectra of cadmium yellow Schmincke normalized to the band with a maximum at 2917 cm−1 assigned to C-H groups are presented. During the thermal degradation of cadmium, a yellow increase in the intensity of the band with a maximum at 1630 cm−1 assigned to COO- groups was observed. The result supports the use of Arabic gum with beef bile evaporation and oxidation of the remnants. A similar trend can be observed for cadmium yellow light degraded, however, alterations in the strength of the bands denoting changes are less pronounced. After 4 years of conditioning, a decreased intensity of bands assigned to C–H and COO- groups was observed. These results indicated that Arabic gum evaporation occurred.

Fig. 4: ATR FTIR spectra of ultramarine Schmincke normalized to a band originating from Si-OH groups with a maximum at 988 cm−1 and cadmium yellow Schmincke normalised to a band with a maximum at 2917 cm−1 assigned to C-H groups.Fig. 4: ATR FTIR spectra of ultramarine Schmincke normalized to a band originating from Si-OH groups with a maximum at 988 cm−1 and cadmium yellow Schmincke normalised to a band with a maximum at 2917 cm−1 assigned to C-H groups.The alternative text for this image may have been generated using AI.

a, d Thermally aged, T = 120 °C, b, e light aged, c, f conditioned for 4 years, respectively.

Figure 5 shows the FTIR spectra of ultramarine blue and cadmium yellow RestaurArte. To visualize the chemical changes that occur during the degradation process, differential spectra were obtained.

Fig. 5: ATR FTIR spectra of ultramarine RestaurArte normalized to a band originating from Si-OH groups with a maximum at 986 cm−1 and cadmium yellow RestaurArte normalised to a band with a maximum at 2916 cm−1 assigned to C-H groups.Fig. 5: ATR FTIR spectra of ultramarine RestaurArte normalized to a band originating from Si-OH groups with a maximum at 986 cm−1 and cadmium yellow RestaurArte normalised to a band with a maximum at 2916 cm−1 assigned to C-H groups.The alternative text for this image may have been generated using AI.

a, d Thermally aged, T = 120 °C, b, e light aged, c, f conditioned for 4 years, respectively.

The differential FTIR spectra of the ultramarine blue RestaurArte were normalized to the band with a maximum at 986 cm−1 originating from Si-OH (Fig. 6a–c) and normalized to the band with a maximum at 2916 cm-1 assigned to the C–H vibration (Fig. 6d–f). During thermal degradation, the intensity of the band attributed to C-H groups decreased (Fig. 5a). Concurrently, the intensity of the band with a maximum at 1738 cm−1, originating from C=O groups, increased (Fig. 6d). The results demonstrated that the polycyclohexanone resin, when combined with ethanol and white spirit, underwent evaporation, resulting in the formation of partially oxidized remnants. In contrast, a different phenomenon was observed for light degradation. A slight decrease in the intensity of the band due to the C-H groups (Fig. 6b) is indicative of the evaporation of the polycyclohexanone resin. Conversely, the increase in the intensity of the C=O band is more pronounced (Fig. 6e), which suggests that the oxidation process plays a significant role in this case After 4 years of conditioning, a decrease in the intensity of the band due to C–H was mainly visible (Fig. 6c, f), which implies that polycyclohexanone resin evaporation was the dominant process.

Fig. 6: Differential FTIR spectra of ultramarine blue RestaurArte normalized to the band originating from Si-OH groups with a maximum at 986 cm−1 and ultramarine blue RestaurArte normalised to the band assigned to C-H groups with a maximum at 2916 cm−1.Fig. 6: Differential FTIR spectra of ultramarine blue RestaurArte normalized to the band originating from Si-OH groups with a maximum at 986 cm−1 and ultramarine blue RestaurArte normalised to the band assigned to C-H groups with a maximum at 2916 cm−1.The alternative text for this image may have been generated using AI.

a, d Thermally aged, T = 120 °C, b, e light aged, c, f conditioned for 4 years, respectively.

Figure 7 presents differential FTIR spectra of cadmium yellow RestaurArte normalized to a band with a maximum at 2916 cm−1 assigned to C-H groups. The thermally degraded cadmium yellow exhibited a large increase in the band with a maximum at 1738 cm−1 originating from C=O groups (Fig. 7a), which indicates the loss of polycyclohexanone resin, with the remaining material undergoing partial oxidation. During light degradation of cadmium yellow RestaurArte, a significantly smaller increase in the intensity of the band due to C=O groups was observed (Fig. 7b). This observation indicated that the primary phenomenon was oxidation. Cadmium yellow RestaurArte after 4 years of conditioning exhibited a similar trend of changes in intensity of band attributed to C=O vibrations as thermally aged paint (Fig. 7c) indicating that polycyclohexanone resin was lost and that the remnants were partially oxidized.

Fig. 7: Differential FTIR spectra of cadmium yellow RestaurArte normalized to a band originating from C-H groups with a maximum at 2916 cm−1.Fig. 7: Differential FTIR spectra of cadmium yellow RestaurArte normalized to a band originating from C-H groups with a maximum at 2916 cm−1.The alternative text for this image may have been generated using AI.

a Thermally aged, T = 120 °C, b light aged, and c conditioned for 4 years.

In Fig. 8 FTIR spectra of ultramarine blue and cadmium yellow Rembrandt are presented. Differential spectra are used to visualize chemical changes during degradation.

Fig. 8: ATR FTIR spectra of ultramarine Rembrandt normalized to a band originating from Si-OH groups with a maximum at 984 cm−1 and cadmium yellow Rembrandt normalised to a band with a maximum at 2914 cm−1 assigned to C-H groups.Fig. 8: ATR FTIR spectra of ultramarine Rembrandt normalized to a band originating from Si-OH groups with a maximum at 984 cm−1 and cadmium yellow Rembrandt normalised to a band with a maximum at 2914 cm−1 assigned to C-H groups.The alternative text for this image may have been generated using AI.

a, d Thermally aged, T = 120 °C, b, e light aged, c, f conditioned for 4 years, respectively.

Figure 9 shows the differential FTIR spectra of the ultramarine blue Rembrandt normalized to the band with a maximum at 984 cm−1 assigned to Si-OH groups (Fig. 9a–c) and normalized to the band with a maximum at 2914 cm−1 assigned to the C–H vibration (Fig. 9d–f). During the thermal degradation of the ultramarine blue, a decrease in the intensity of the band due to C–H groups occurred. Conversely, an increase in the intensity of the band with a maximum at 1706 cm−1, originating from C=O groups, was proportional to the decrease in the intensity of the band due to C–H groups (Fig. 9a). This observation suggests an equilibrium between the evaporation and oxidation of polycyclohexanone resin with odorless turpentine and the addition Talens 004 varnish. A similar trend can be observed for the degradation of ultramarine blue Rembrandt light (Fig. 9b, e). In this instance, the most significant alterations are evident at the outset of the ageing process. After 4 years of conditioning, a decrease in the intensity of the band due to C–H groups was observed. Concurrently, no change in the intensity of the band due to C=O groups was observed, which serves to corroborate the hypothesis that polycyclohexanone resin evaporation is the sole process occurring.

Fig. 9: Differential FTIR spectra of ultramarine blue Rembrandt normalized to the band originating from Si-OH groups with a maximum at 986 cm−1 and ultramarine blue Rembrandt normalised to the band assigned to C-H groups with a maximum at 2914 cm−1.Fig. 9: Differential FTIR spectra of ultramarine blue Rembrandt normalized to the band originating from Si-OH groups with a maximum at 986 cm−1 and ultramarine blue Rembrandt normalised to the band assigned to C-H groups with a maximum at 2914 cm−1.The alternative text for this image may have been generated using AI.

a, d Thermally aged, T = 120 °C, b, e light aged, c, f conditioned for 4 years, respectively.

Figure 9a–c shows the differential FTIR spectra of cadmium yellow Rembrandt normalized to the band with a maximum at 2914 cm−1 assigned to the C–H vibration. Cadmium yellow thermally degraded manifests a large increase in the intensity of the band with a maximum at 1706 cm−1 assigned to C=O groups (Fig. 10a), suggesting considerable depletion of polycyclohexanone resin with odorless turpentine and Talens 004 varnish addition, along with partial oxidation of residual materials. The observed reduction in the intensity of the band due to C=O groups during light degradation (Fig. 10b) is indicative of the predominance of the oxidizing process. A parallel can be drawn with the ultramarine blue Rembrandt in cadmium yellow, where the most pronounced alterations are evident at the outset of the ageing process. After 4 years of conditioning cadmium yellow Rembrandt increase of the intensity of the band due to C=O vibrations was not observed (Fig. 10c). The outcome of the analysis demonstrated that no alterations were observed.

Fig. 10: Differential FTIR spectra of cadmium yellow Rembrandt normalized to the band originating from C-H groups with a maximum at 2914 cm−1.Fig. 10: Differential FTIR spectra of cadmium yellow Rembrandt normalized to the band originating from C-H groups with a maximum at 2914 cm−1.The alternative text for this image may have been generated using AI.

a Thermally aged, T = 120 °C, b light aged, c conditioned for 4 years.

In Fig. 11 the FTIR spectra of ultramarine blue and cadmium yellow Gamblin are given. To facilitate the observation of changes, differential spectra were obtained.

Fig. 11: ATR FTIR spectra of ultramarine Gamblin normalized to a band originating from Si-OH groups with a maximum at 1008 cm−1 and cadmium yellow Gamblin normalised to a band with a maximum at 2953 cm−1 assigned to C-H groups.Fig. 11: ATR FTIR spectra of ultramarine Gamblin normalized to a band originating from Si-OH groups with a maximum at 1008 cm−1 and cadmium yellow Gamblin normalised to a band with a maximum at 2953 cm−1 assigned to C-H groups.The alternative text for this image may have been generated using AI.

a, d Thermally aged, T = 120 °C, b, e light aged, c, f conditioned for 4 years, respectively.

Differential FTIR spectra of ultramarine blue Gamblin were normalized to band with a maximum at 1008 cm−1 originating from Si-O-Si groups (Fig. 12a–c) and normalized to a band with a maximum at 2953 cm−1 assigned to the C–H vibration (Fig. 12d–f). The spectra of thermally degraded ultramarine blue Gamblin demonstrated a notable decrease in intensity, which can be attributed to the substantial depletion of the Laropal A81 resin. Concurrently, the increase in the intensity of the band with a maximum at 1726 cm−1, attributed to C=O groups, is considerably less pronounced (Fig. 12d), which indicates that the loss of the Laropal A81 resin occurs mainly. The same trend of changes in the intensity of bands originating from C–H and C=O groups was observed during light degradation (Fig. 12b, e) and 4 years of conditioning (Fig. 12c, f). However, the intensity of these changes is significantly reduced. In all the cases, the most significant alterations are observable at the outset of the degradation process.

Fig. 12: Differential FTIR spectra of ultramarine blue Gamblin normalized to the band originating from Si-OH groups with a maximum at 1008 cm−1 and ultramarine blue Gamblin normalised to the band assigned to C-H groups with a maximum at 2953 cm−1Fig. 12: Differential FTIR spectra of ultramarine blue Gamblin normalized to the band originating from Si-OH groups with a maximum at 1008 cm−1 and ultramarine blue Gamblin normalised to the band assigned to C-H groups with a maximum at 2953 cm−1The alternative text for this image may have been generated using AI.

a, d Thermally aged, T = 120 °C, b, e light aged, c, f conditioned for 4 years, respectively.

The differential FTIR spectra of cadmium yellow Gamblin normalized to a band with a maximum at 2953 cm−1 originating from C-H groups are presented in Fig. 13a–c. The same trend is observed during thermal (Fig. 13a) and light (Fig. 13b) degradation, namely a significant increase in the intensity of the band with a maximum at 1726 cm−1, which is attributed to C=O groups. The results indicate that the loss of Laropal A81 resin plays a dominant role in oxidation, similar to that observed with ultramarine blue Gamblin. Furthermore, the most significant changes were observed at the outset of the ageing process. The increase in the intensity of the band attributed to C=O groups after 4 years of conditioning (Fig. 13c) in the spectrum of cadmium yellow Gamblin was markedly less pronounced. This phenomenon serves to illustrate the preponderant role of the oxidizing process in this particular instance.

Fig. 13: Differential FTIR spectra of cadmium yellow Gamblin normalized to the band originating from C-H groups with a maximum at 2953 cm−1.Fig. 13: Differential FTIR spectra of cadmium yellow Gamblin normalized to the band originating from C-H groups with a maximum at 2953 cm−1.The alternative text for this image may have been generated using AI.

a Thermally aged, T = 120 °C, b light aged, c conditioned for 4 years.

FTIR spectra of ultramarine blue and cadmium yellow Kremer based on the same binder as Gamblin are depicted in Fig. 14. A comprehensive illustration of the chemical alterations that occur during the degradation process is provided in the differential spectra.

Fig. 14: ATR FTIR spectra of ultramarine Kremer normalized to a band originating from Si-OH groups with a maximum at 1053 cm−1 and cadmium yellow Kremer normalised to a band with a maximum at 2969 cm−1 assigned to CH groups.Fig. 14: ATR FTIR spectra of ultramarine Kremer normalized to a band originating from Si-OH groups with a maximum at 1053 cm−1 and cadmium yellow Kremer normalised to a band with a maximum at 2969 cm−1 assigned to CH groups.The alternative text for this image may have been generated using AI.

a, d Thermally aged, T = 120 °C, b, e light aged, c, f conditioned for 4 years, respectively.

The differential FTIR spectra of the ultramarine blue Kremer normalized to the band with a maximum at 1053 cm−1 assigned to Si-OH groups are presented in Fig. 15a–c. Spectra normalized to the band with a maximum at 2969 cm−1 originating from the C–H groups are presented in Fig. 15d–f. The intensity of the changes indicated by the bands is considerably less visible in the spectra than that of ultramarine Gamblin, yet the trends are similar. Both the ultramarine blue Kremer thermally (Fig. 15a, d) and light degraded (Fig. 15b, e) exhibited notable decreases in the intensity of the band assigned to the C–H vibration and increases in the intensity of the band with a maximum at 1730 cm−1 originating from the C=O groups. This evidence corroborates the substantial loss of the Laropal A81 resin. The difference in comparison to Gamblin is even the intensity of changes during degradation. After 4 years of conditioning (Fig. 15c, f), a decrease in the intensity of the band due to C–H groups was observed, which indicated that the loss of the Laropal A81 resin played the main role.

Fig. 15: Differential FTIR spectra of ultramarine Kremer normalized to the band originating from Si-O-Si groups with a maximum at 1053 cm-1.Fig. 15: Differential FTIR spectra of ultramarine Kremer normalized to the band originating from Si-O-Si groups with a maximum at 1053 cm-1.The alternative text for this image may have been generated using AI.

a Thermally aged, T = 120 °C, b light aged, c conditioned for 4 years, and ultramarine Kremer normalized to the band assigned to C-H groups with a maximum at 2969 cm-1, d thermally aged, T = 120 °C, e light aged, f conditioned for 4 years.

The differential FTIR spectra of the cadmium yellow Kremer normalized to the band with a maximum at 2969 cm−1 originating from C-H groups are presented in Fig. 16. The same trend is observed during thermal (Fig. 16a) and light (Fig. 16b) degradation: a significant increase in the intensity of the band with a maximum at 1730 cm−1, which is assigned to C=O groups. This phenomenon was also observed for the cadmium yellow Gamblin (Fig. 13). This indicates that the loss of the Laropal A81 resin plays a dominant role in oxidation. After 4 years of conditioning, (Fig. 16c) the increase in the intensity of the band assigned to the C=O groups was less pronounced. This suggests that oxidation represents a primary process in this instance.

Fig. 16: Differential FTIR spectra of cadmium yellow Kremer normalized to the band originating from C-H groups with a maximum at 2969 cm−1.Fig. 16: Differential FTIR spectra of cadmium yellow Kremer normalized to the band originating from C-H groups with a maximum at 2969 cm−1.The alternative text for this image may have been generated using AI.

a Thermally aged, T = 120 °C, b light aged, c conditioned for 4 years.

In the context of thermal degradation, FTIR spectroscopy measurements have been shown to indicate the evaporation of gum Arabic in the case of watercolors and the oxidizing process in the case of polycyclohexanone and Laropal A81 resins. In the case of paints subjected to light degradation, oxidizing processes marked by the creation of carbonyl groups (C=O) have been shown to play a primary role. The specific degradation process varies depending on the type of paint during the 4-year conditioning period. In the case of paints based on ketone and Laropal A81 resin, the process is either mainly binder evaporation and a lesser extent oxidation which is mainly observed in the case of watercolors. The stability of the paint depends on the type of pigment: ultramarine blue is less stable than cadmium yellow due to a change in the mechanical properties of the paint.

Color durability by spectrophotometry

The stability of the color was evaluated by a spectrophotometric technique based on the CIELAB model. Figures 16–21 present the changes in the color of the ultramarine blue and cadmium yellow paint.

Changes in the colors of the ultramarine blue and cadmium yellow Leningrad paints according to the chromatic coefficients available in Table S1 in the Supplementary Information file are presented in Fig. 17. In the case of the thermally and light degraded paint samples, the changes in the ultramarine blue color (Fig. 17a) were faster and more intense than those in the cadmium yellow (Fig. 17b) and could be observed by an unexperienced observer. Because the ultramarine sample fell out of the glass it was not possible to perform all the measurements. The conditioned ultramarine blue (Fig. 17a) exhibited considerably more pronounced color alterations than the thermal and light degraded paints. The changes in the color of the conditioned cadmium yellow (Fig. 17b) are analogous to those observed in the light degraded ultramarine blue and can be observed by experienced observers.

Fig. 17: Paint colour changes during thermal, light, and conditioned for 4 years.Fig. 17: Paint colour changes during thermal, light, and conditioned for 4 years.The alternative text for this image may have been generated using AI.

a Ultramarine blue Leningrad and b cadmium yellow Leningrad.

The total color alterations are shown in Fig. 18 based on the chromatic coefficients of ultramarine blue and cadmium yellow and are included in Table S2. The intensity of the color change in the thermally degraded paints was greater for ultramarine blue than for cadmium yellow, indicating the presence of two different colors. Ultramarine blue and cadmium yellow during light degradation and after 4 years of conditioning exhibited more pronounced color changes than did those observed during thermal degradation and can be observed by inexperienced observers. In general, Leningrad (Fig. 17) has a more stable color than that of Schmincke (Fig. 18).

Fig. 18: Paint colour changes during thermal, light, and conditioned for 4 years.Fig. 18: Paint colour changes during thermal, light, and conditioned for 4 years.The alternative text for this image may have been generated using AI.

a Ultramarine blue Schmincke and b cadmium yellow Schmincke.

The chromatic coefficients collected in Table S3 and available in the Supplementary Information file are used to visualize the changes in the color of the ultramarine blue and cadmium yellow RestaurArte paint in Fig. 19. The most notable alterations are evident in the thermally degraded ultramarine blue (Fig. 19a) and conditioned ultramarine blue and cadmium yellow (Fig. 19b), indicating two different colors. The cadmium yellow thermally aged specimens (Fig. 19b) exhibit a comparable color alteration to that observed in the thermally aged specimens at the outset. light degraded paints have significantly fewer color changes and can be noticed by inexperienced observers.

Fig. 19: Paint colour changes during thermal, light, and conditioned for 4 years.Fig. 19: Paint colour changes during thermal, light, and conditioned for 4 years.The alternative text for this image may have been generated using AI.

a Ultramarine blue RestaurArte and b cadmium yellow RestaurArte.

Figure 20 shows the changes in the color of ultramarine blue and cadmium yellow Rembrandt based on the chromatic coherence data collected in Table S4 in the Supplementary Information file. The greatest color change was observed for thermal and light aged ultramarine blue (Fig. 20a), especially at the beginning of the ageing process, and for the conditioned cadmium yellow (Fig. 20b), indicating two different colors. The changes in the colors of the ultramarine blue after 4-years of conditioning are comparable to those of the cadmium yellow, which underwent thermal and light degradation at the outset and can be observed only by experienced observers. The color changes observed in the ultramarine blue after 4-years of conditioning (Fig. 20a) can be observed by an inexperienced observer. In general, the color of Rembrandt (Fig. 20) was slightly more stable than that of RestaurArte (Fig. 19).

Fig. 20: Paint colour changes during thermal, light, and conditioned for 4 years.Fig. 20: Paint colour changes during thermal, light, and conditioned for 4 years.The alternative text for this image may have been generated using AI.

a Ultramarine blue Rembrandt and b cadmium yellow Rembrandt.

The intensity of the changes in the colors of ultramarine blue and cadmium yellow Gamblin according to the chromatic coefficients in Table S5 available in the Supplementary Information file are shown in Fig. 21. The color changes of the thermally degraded cadmium yellow (Fig. 21b) are significantly less visible than those of the thermally degraded and conditioned ultramarine blue (Fig. 21a) an indicate two different colors. The degree of color alteration observed in the ultramarine blue (Fig. 21a) and cadmium yellow light degraded (Fig. 21b) specimens was comparable to that of cadmium yellow after 4 years of conditioning and could be observed only by experienced observers. Changes in the color of cadmium yellow (Fig. 21b) are mostly visible in thermally aged paint and are noticeable only for an experienced observer.

Fig. 21: Paint colour changes during thermal, light, and conditioned for 4 years.Fig. 21: Paint colour changes during thermal, light, and conditioned for 4 years.The alternative text for this image may have been generated using AI.

a Ultramarine blue Gamblin and b cadmium yellow Gamblin.

The changes in the colors of the ultramarine blue and cadmium yellow Kremer described by the chromatic coefficients are available in Table S6 in the Supplementary Information file and are presented in Fig. 22. In general, ultramarine blue (Fig. 22a) exhibited greater color shifts than cadmium yellow (Fig. 22b). The changes in the colors of the ultramarine blue after 4 years of conditioning (Fig. 22a) are comparable to those of the ultramarine blue that underwent thermal and light degradation at the outset of the degradation process and indicate two different colors. The degree of color change in the color of cadmium yellow was relatively consistent across all the types of paints (Fig. 22b) and was noticeable only for experienced observers. The general conclusion is that Kremer resin paint has slightly more stable color than Gamblin despite both paints containing the same binder, Laropal A81 resin.

Fig. 22: Paint colour changes during thermal, light, and conditioned for 4 years.Fig. 22: Paint colour changes during thermal, light, and conditioned for 4 years.The alternative text for this image may have been generated using AI.

a Ultramarine blue Kremer and b cadmium yellow Kremer.

The spectrophotometric measurements of color stability indicate that paints based on Laropal A81 resin exhibit the most stable color and are the optimal choice for the conservation of paintings. Furthermore, ultramarine blue demonstrates a more pronounced color change than cadmium yellow, with color changes towards yellow might be related to the an increase in the quantity of yellow radical S2− chromophores22.

Surface properties by contact angle measurements

The contact angle is a property of the paint surface. The standard is used to determine the choice of solvent for removing old paint.

The contact angle values corresponding to the paint surface are presented in Table 2. Leningrad and Schmincke watercolor paints, in their original state, display high hydrophilicity and are characterized by a low contact angle. In the case of Leningrad ultramarine, it was not possible to obtain measurements following thermal and light degradation, as the sample had undergone complete degradation and had fallen off the glass. It is evident that RestaurArte and Rembrandt polycyclohexanone resin-based paints exhibit a markedly hydrophobic character. During the process of thermal and light degradation, the contact angle decreased, which signifies that the paint has become increasingly hydrophilic. The minimal alterations are discernible in the conditioned paints, which demonstrate a comparatively elevated hydrophobicity. The lowest degree of hydrophilicity was exhibited by the resin paints from Gamblin and Kremer. All the samples, both new and aged, demonstrated high contact angles, which attested to their high hydrophobicity. The contact angle changes observed across all degradation pathways (thermal, light and 4-year conditioning) are insignificant.

Table 2 Contact angle values obtained with distilled water

The contact angle measurements indicate the most increase in hydrophilicity of the paints during light degradation, which corresponds with chemical changes consisting of oxidation. Paints subjected to thermal degradation and 4-year conditioning also manifest an increase in hydrophilicity but to a lesser extent than light degraded samples. Paints based on Laropal A81 and cyclohexanone resins require the use of an organic solvent for removal, whereas watercolors can be removed with water.

Pigments characterization by electron paramagnetic resonance spectroscopy

Although electron paramagnetic resonance (EPR) is not a widely utilized technique among conservators, historians, or painting researchers, it has proven effective in examining rock and wall paintings47,48, as well as individual pigments23,34. In the case of ultramarine pigments, all the EPR spectra contained the strong isotropic lines with giso = 2.0286 ± 0.0005 and a Lorentzian lineshape, and a representative spectrum is given in Fig. 23. This signal is typical for S3− radical centers in the sodalite mineral Na8[A16Si6O24]C12, where the sulfur radicals substitute chloride ions in the face centered lattice49,50,51,52.

Fig. 23Fig. 23The alternative text for this image may have been generated using AI.

X-band EPR spectra of Leningrad blue paint with ultramarine pigments registered at room temperature: experimental (black line) and simulated (red dashed).

In Fig. 24 EPR spectra in the range of 50–7050 G for all the investigated samples before and after thermal degradation at 120 °C are presented. As previously mentioned, the signal is very stable and persists even after 77 days of treatment at this temperature. This finding reinforces the assumption that sodalite remains stable and that IR spectra can be normalized to the band at approximately 1000 cm−1, which is attributed to Si-OH or Si-O-Si groups.

Fig. 24: X-band spectra of the ultramarine paint samples before and after thermal degradation at 120 °C.Fig. 24: X-band spectra of the ultramarine paint samples before and after thermal degradation at 120 °C.The alternative text for this image may have been generated using AI.

Leningrad (a), Schmincke (b), RestaurArte (c), Rembrandt (d), Gamblin (e), Kremer (f).

However, in the wide-range EPR spectra, in addition to the narrow signal from the S3− radicals described above, additional signals are visible, especially in the case of the RestaurArte paint (Fig. 25a).

Fig. 25: X-band EPR spectra of ultramarine paints.Fig. 25: X-band EPR spectra of ultramarine paints.The alternative text for this image may have been generated using AI.

a Full range, b magnified part of the same spectra.

The differences can be seen more clearly in Fig. 25, where the spectra are magnified. These lines can be assigned to impurities, the most likely originating from iron species15.

The results obtained by the EPR method indicate that the pigment (lapis lazuli) used in the blue colors has a very high thermal stability. Color changes due to thermal ageing are mainly due to evaporation and degradation of the organic components and not to degradation of the lazurite mineral. In addition, the EPR spectra contained additional signals from impurities present in the pigment, and these varied depending on the manufacturer. The quantity and nature of the contamination are specific to the manufacturer of the paint and can be used to identify its origin.